FKM-65B20
| Nnweta: | |
|---|---|
| Ọnụọgụ: | |
A na-ewu ọkpụkpụ azụ polymer site na vinylidene fluoride (VDF) , hexafluoropropylene (HFP) na tetrafluoroethylene (TFE) na nha 40/30/30, na-enye ọdịnaya fluorine kachasị elu dị na FKM azụmahịa . Matriks fluorocarbon a siri ike na-emepụta ihe mgbochi ike dị ala dị ala (<18mN m⁻¹) nke na-achụpụ mmanụ ndị na-abụghị polar hydrocarbons , polar ester oil , yana ihe mgbakwunye ike dị ka methanol ma ọ bụ biodiesel. Sistemụ ọgwụgwọ bisphenol-AF na-ekpochapụ peroxide na-ekpochapụ mgbakasị mgbawa mgbe ọgwụgwọ gasịrị, na-enye > 20 MPa ike ike na 35 kN m⁻¹ ike akwa akwa ọbụlagodi 1,000 h @ 200 Celsius . Nsonaazụ bụ ngwakọta nke na-adị ndụ silicon na HNBR site na 3 × n'otu envelopu thermal ka ọ na-ejigide <3 % olu na-aza na mmanụ ntụaka IRM903.
| Ule | Ule | FKM-65B20 Uru | Industry Benchmark |
|---|---|---|---|
| Njupụta | ASTM D792 | 1.82 g cm | 1.80–1.85 |
| Isi ike | ASTM D2240 | 75 ± 3 Oke A | 70–80 |
| Ike ọdụdọ | ASTM D412 | 20.5 MPa | > 18 MPa |
| Elongation @ ezumike | ASTM D412 | 230% | > 180% |
| Ntọala mkpakọ (200 °C × 70 h) | ASTM D395 | 18% | <25% |
| Nkịta dị ala | ASTM D2137 | -25 Celsius C | -20 Celsius C |
| Mpịakọta na mmanụ ọkụ C (23 Celsius C × 70 h) | ASTM D471 | 1.2% | <5% |
| Ịka nká na ikuku 250 °C × 70 h | ASTM D573 | Mgbanwe nkwụsị -5% | <-15% |
Turbocharger Systems
Ọwa ikuku na diaphragms valve na-agbapụ nke na-ahụ elu 260 Celsius C n'okpuru ngwa ngwa siri ike.
Wastegate actuator akara na- eguzogide mmanụ 5W-30 sịntetik + soot.
Mmanụ na SCR sekit
O-mgbanaka ntụ ntụ na -emechi mmanụ dizel mmanya 350.
AdBlue (DEF) injector akàrà ebe FKM-65B20 's dị ala extractables na-egbochi crystallization rụrụ arụ.
Injin & nnyefe
Igwe nju oyi mmanụ ekpughere na mmanụ 150 Celsius C + ịma jijiji.
E-motor ụlọ grommets na PHEVs ebe electrolyte vapors na-awakpo ọkọlọtọ elastomers.
Chassis & breeki
ESP hydraulic accumulator eriri afọ chọrọ <0.1% mmanụ ọkụ.
Igwe nkwusioru ikuku na-eguzogide ozone, nnu okporo ụzọ, na mmiri breeki.
Ụdị ngwakọta : slab, warara, ma ọ bụ pellet agwakọtara tupu oge eruo maka mkpakọ, nyefe, ma ọ bụ ịkpụzi injection.
Usoro ọgwụgwọ a na-ahụkarị : 5 min @ 170 Celsius C pịa + ọgwụgwọ emechara 2 h @ 200 Celsius C (ikuku) ma ọ bụ 30 min @ 230 Celsius C uzuoku maka <1 % ewepụtara.
Akụkụ slab : 300 mm × 300 mm × 10 mm (omenala 2-30 mm).
Ndụ nchekwa : 12 ọnwa @ ≤ 25 Celsius C na aluminom-foil / PE akpa abụọ; nitrogen-flushed iji gbochie ikuku oxidative.
ISO 9001: 2015 & IATF 16949: 2016 ihe ọkụkụ na-agbakọta akwụkwọ.
REACH & RoHS 3.0 nkwupụta zuru oke (SVHC <0.1%).
Akuko Ule SGS - akwa, nhazi mkpakọ, mmanụ ọkụ (budata PDF).
Nkwupụta okwu ịnweta mgbagha - ị nweta enweghị DRC.
| Order Ụdị | MOQ | Lead Time | Packaging | Incoterm |
|---|---|---|---|---|
| Ngwakọta ngwaahịa | 25 n'arọ | 7-10 ụbọchị | Akpa PE + katọn | EXW Shenzhen |
| Agba/ike siri ike | 250 n'arọ | 3-4 izu | Iberibe ekpuchiri oghere | FOB Shenzhen |
| Pelletized maka extrusion | 500 n'arọ | 4-5 izu | Akpa foil 25kg | Ụlọ ọrụ CIF Hamburg |
Ejikọtara ya na eriri igwe anaghị agba nchara
maka eriri turbocharger kpughere > 200 Celsius C , abụọ gaskets FKM-65B20 na eriri eriri 316 SS nwere akara -80 Celsius C ruo + 538 Celsius C maka sistemu mkpuchi kemịkalụ zuru oke..