An gina kashin baya na polymer daga vinylidene fluoride (VDF) , hexafluoropropylene (HFP) da tetrafluoroethylene (TFE) a cikin daidaitaccen rabo na 40/30/30, yana samar da mafi girman abun ciki na fluorine a cikin FKM na kasuwanci . Wannan matrix fluorocarbon matrix yana haifar da shingen makamashi mara ƙarancin ƙarfi (<18 mN m⁻¹) wanda ke korar da ba na polar hydrocarbons , polar ester oils , da ƙari mai ƙarfi kamar methanol ko biodiesel. The peroxide-scavenging bisphenol-AF tsarin magani yana kawar da ɓarna bayan-cure embrittlement, bada > 20 MPa ƙarfi ƙarfi da 35 kN m⁻¹ ƙarfin hawaye ko da bayan 1,000 h @ 200 °C . Sakamakon shine fili wanda ya wuce silicone da HNBR ta 3 × a cikin ambulaf ɗin thermal iri ɗaya yayin da yake riƙe <3 % ƙarar ƙarar man fetur na IRM903.
| Kaya | Hanyar Gwajin | FKM-65B20 Alamar Masana'antar | ƙimar ƙimar |
|---|---|---|---|
| Yawan yawa | Saukewa: ASTM D792 | 1.82 g cm³ | 1.80-1.85 |
| Tauri | Saukewa: ASTM D2240 | 75 ± 3 Gabar A | 70-80 |
| Ƙarfin Ƙarfi | Saukewa: ASTM D412 | 20.5 MPa | > 18 MPa |
| Tsawaitawa @ Hutu | Saukewa: ASTM D412 | 230% | > 180% |
| Saitin Matsi (200 °C × 70 h) | Saukewa: ASTM D395 | 18% | <25% |
| Ƙarƙashin zafi | Saukewa: ASTM D2137 | -25 ° C | -20 °C |
| Ƙarar Ƙarar Man Fetur C (23 °C × 70 h) | Saukewa: ASTM D471 | 1.2% | <5% |
| Tsufa a cikin iska 250 °C × 70 h | Saukewa: ASTM D573 | Canjin juzu'i - 5% | <-15% |
Turbocharger Systems
Cajin-iska bututu da busa-off bawul diaphragms cewa ganin 260 ° C kololuwa a karkashin m hanzari.
Wastegate actuator hatimin tsayayya da roba 5W-30 mai + soot.
Fuel & SCR kewaye
O-rings allura kai tsaye suna rufe man dizal bar 350.
AdBlue (DEF) injector hatimi inda FKM-65B20 's low extractables hana crystallization fouling.
Injin & Watsawa
Gaskets mai sanyaya mai da aka fallasa ga mai 150 ° C + girgiza.
E-motor gidaje grommets a cikin PHEVs inda electrolyte vapors hari daidaitattun elastomers.
Chassis & Birki
ESP hydraulic accumulator bladders suna buƙatar <0.1% permeation na man fetur.
Dakatarwar iska tana jure wa ozone, gishirin hanya, da ruwan birki.
Form ɗin Haɗaɗɗen : Tsari, tsiri, ko pellet wanda aka riga aka haɗa don matsawa, canja wuri, ko gyare-gyaren allura.
Yawan Maganin Magani : Minti 5 @ 170 °C latsa + magani bayan 2 h @ 200 °C (iska) ko 30 min @ 230 °C tururi don <1 % abubuwan cirewa.
Girman Slab : 300 mm × 300 mm × 10 mm (al'ada 2-30 mm).
Rayuwar Shelf : watanni 12 @ ≤ 25 ° C a cikin aluminum-foil / PE biyu; jakar nitrogen-flushed don hana oxidative kumburi.
ISO 9001: 2015 & IATF 16949: 2016 ƙwararrun masana'anta.
REACH & RoHS 3.0 cikakken sanarwa (SVHC <0.1%).
Rahoton Gwajin SGS - hawaye, saitin matsawa, kumburin mai (zazzage PDF).
Bayanin Ma'adinan Rikici -Ma'adinan DRC kyauta.
| Nau'in | MOQ | Gubar Lokacin | Marufi | Incoterm |
|---|---|---|---|---|
| Haɗin Hannu | 25 kg | 7-10 kwanaki | PE jakar + kartani | EXW Shenzhen |
| Launi/Tauri na Musamman | 250 kg | 3-4 makonni | Tsiri mai rufewa | FOB Shenzhen |
| Pelletized don Extrusion | 500 kg | 4-5 makonni | 25 kilogiram na foil bags | CIF Hamburg |
Bundle tare da Bakin Karfe Cable Ties
Don kayan aikin turbocharger da aka fallasa zuwa > 200 ° C , biyu FKM-65B20 gaskets tare da haɗin kebul ɗin mu na 316 SS wanda aka ƙididdige -80 °C zuwa +538 °C don cikakken tsarin rufewa na thermal-chemical.