FV9400
Herchy
| Availability: | |
|---|---|
| Quantity: | |
Items |
Indicators |
||||||
Grades |
FV9430 |
FV9440 |
FV9450 |
FV9460 |
FV9470 |
FV9480 |
|
Appearance |
Milky white translucent |
Yellowish |
|||||
Specific Gravity/ g/cm3 |
ASTM D792 |
1.38 |
1.41 |
1.42 |
1.43 |
1.45 |
1.47 |
Hardness/shoreA |
ASTM D2240 |
28 |
40 |
48 |
60 |
70 |
80 |
Tensile Strength/MPa |
ASTM D412 |
10.2 |
9.5 |
9.5 |
10.2 |
9.9 |
8.1 |
Elongation At Break /% |
ASTM D412 |
485 |
494 |
363 |
296 |
241 |
159 |
Tear Strength/KN/m |
ASTM D624-B |
18 |
26 |
19 |
22 |
21 |
16 |
Compression Set(177℃*22h) |
ASTM D395 |
9 |
8 |
8 |
7 |
8 |
9 |
Resilience/% |
ASTM D1054 |
41 |
35 |
46 |
40 |
37 |
39 |
*Heat Resistance |
Hardness change /shore A |
+2 |
+2 |
+3 |
+2 |
+2 |
+3 |
Tensile strength change, % |
-18 |
-17 |
-21 |
-25 |
-20 |
-19 |
|
Elongation at break change, % |
-19 |
-16 |
-18 |
-21 |
-16 |
-15 |
|
Fuel C Volume Change/% 23℃/72h |
ASTM D471 |
+22 |
+19 |
+18 |
+19 |
+19 |
+19 |
Curing Condition |
Add 0.7 parts of bis(2+5), one stage vulcanisation 170℃×15min, two stage vulcanisation: 200℃×4h. |
||||||
Recommended actions:
It's suggested to utilize 0.6 to 1 part of bisdipenta chemical agent for vulcanization (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane).
Customers should choose the most appropriate temperature and time for curing based on the product's size and method of curing.
Product packaging:
This product is not dangerous, it's instead composed of cardstock, plastic, and 10 kilograms per bag, 2 bags per box.
Age of storage:
This product has a cold flow capacity, the bag should be avoided in order to not have it damaged during transportation or utilization.
Keep in a cool, dry environment with a shelf life of 12 months.