Dzedzeme |
Milky white si me kɔ nyuie |
Dzĩe |
|||||
Nuheŋusẽ Tɔxɛ/ g/cm3 |
ASTM D792 ƒe dɔwɔwɔ |
1.38 |
1.41 |
1.42 |
1.43 |
1.45 |
1.47 |
Sesẽme/ƒutaA |
ASTM D2240 ƒe ƒuƒoƒo |
28 |
40 |
48 |
60 |
70 |
80 |
Tensile Ŋusẽ/MPa |
ASTM D412 ƒe dɔwɔwɔ |
10.2 |
9.5 |
9.5 |
10.2 |
9.9 |
8.1 |
Elongation Le Gbɔɖeme /% . |
ASTM D412 ƒe dɔwɔwɔ |
485 |
494 |
363 |
296 |
241 |
159 |
Aɖatsi ƒe Ŋusẽ/KN/m |
ASTM D624-B ƒe dɔwɔwɔ |
18 |
26 |
19 |
22 |
21 |
16 |
Nutete Ðoɖo(177°C * 22h) |
ASTM D395 ƒe ƒuƒoƒo |
9 |
8 |
8 |
7 |
8 |
9 |
Tenɔnɔ/% |
ASTM D1054 ƒe ƒuƒoƒo |
41 |
35 |
46 |
40 |
37 |
39 |
*Dzoxɔxɔ ƒe Tsitretsitsi |
Sesẽme ƒe tɔtrɔ /ƒuta A |
+2 |
+2 |
+3 |
+2 |
+2 |
+3 |
Tensile ŋusẽ ƒe tɔtrɔ, % . |
-18 |
-17 |
-21 |
-25 |
-20 |
-19 |
|
Elongation le break ƒe tɔtrɔ, % . |
-19 |
-16 |
-18 |
-21 |
-16 |
-15 |
|
Mɔ̃memi C Agbɔsɔsɔme ƒe Tɔtrɔ/% . 23°C/72h ƒe dzoxɔxɔ |
ASTM D471 ƒe dɔwɔwɔ |
+22 |
+19 |
+18 |
+19 |
+19 |
+19 |
Dɔyɔyɔ ƒe Nɔnɔme |
Tsɔ bis(2+5) ƒe akpa 0.7 kpe ɖe eŋu, afɔɖeɖe ɖeka ƒe vulcanisation 170°C×15min, afɔɖeɖe eve ƒe vulcanisation: 200°C×4h. |
||||||
Nuwɔna siwo wokafu:
Wodo susua ɖa be woazã bisdipenta atike ƒe akpa 0.6 va ɖo 1 hena vulcanization (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane).
Ele be asisiwo natia dzoxɔxɔ kple ɣeyiɣi si sɔ wu na dɔyɔyɔ le atike la ƒe lolome kple mɔnu si woatsɔ ada dɔe nu.
Nusiwo wobla ɖe agba me:
Afɔku mele atike sia me o, ke boŋ wotsɔ kakɛ, plastik, kple kilogram 10 le kotoku ɖeka me, kotoku 2 le aɖaka ɖeka me.
Ƒe si wotsɔ dzrae ɖo:
Adzɔnu sia ƒe sisi ƒe ŋutete le vuvɔ me, ele be woaƒo asa na kotokua ale be wòagagblẽ le etsɔtsɔ alo zazã me o.
Dzrae ɖe teƒe si fa miamiamia si me tsi mele o eye wòanɔ anyi ɣleti 12.