FV9400
Herchy
| Ri fhaotainn: | |
|---|---|
| Meud: | |
Nithean |
Comharran |
||||||
Ìrean |
FV9430 |
FV9440 |
FV9450 |
FV9460 |
FV9470 |
FV9480 |
|
coltas |
Milky geal tar-shoilleir |
Buidheach |
|||||
Gravity sònraichte / g / cm3 |
ASTM D792 |
1.38 |
1.41 |
1.42 |
1.43 |
1.45 |
1.47 |
cruas/cladach A |
ASTM D2240 |
28 |
40 |
48 |
60 |
70 |
80 |
Neart tensile/MPa |
ASTM D412 |
10.2 |
9.5 |
9.5 |
10.2 |
9.9 |
8.1 |
Meudachadh aig briseadh / % |
ASTM D412 |
485 |
494 |
363 |
296 |
241 |
159 |
Neart deòir/KN/m |
ASTM D624-B |
18 |
26 |
19 |
22 |
21 |
16 |
Seata teannachaidh (177 ℃ * 22h) |
ASTM D395 |
9 |
8 |
8 |
7 |
8 |
9 |
Fulangas/% |
ASTM D1054 |
41 |
35 |
46 |
40 |
37 |
39 |
* Seasmhachd teas |
Atharrachadh cruas / cladach A |
+2 |
+2 |
+3 |
+2 |
+2 |
+3 |
Atharrachadh neart tensile, % |
-18 |
-17 |
-21 |
-25 |
-20 |
-19 |
|
Leudachadh aig atharrachadh briseadh, % |
-19 |
-16 |
-18 |
-21 |
-16 |
-15 |
|
connadh C Atharrachadh fuaim/% 23 ℃ / 72 h |
ASTM D471 |
+22 |
+19 |
+18 |
+19 |
+19 |
+19 |
Suidheachadh leigheas |
Cuir 0.7 pàirtean de bis (2 + 5), aon ìre vulcanization 170 ℃ × 15min, dà ìre vulcanization: 200 ℃ × 4h. |
||||||
Gnìomhan a thathar a’ moladh:
Thathas a’ moladh pàirt 0.6 gu 1 de àidseant ceimigeach bisdipenta a chleachdadh airson vulcanization (2,5-dimethyl-2,5-bis (tert-butylperoxy) hexane).
Bu chòir do luchd-ceannach an teòthachd agus an ùine as freagarraiche a thaghadh airson leigheas a rèir meud an toraidh agus an dòigh ciùraigidh.
Pacadh toraidh:
Chan eil an toradh seo cunnartach, an àite sin tha e air a dhèanamh suas de stoc cairt, plastaig, agus 10 cileagram gach poca, 2 phoca gach bogsa.
Aois stòraidh:
Tha comas sruthadh fuar aig an toradh seo, bu chòir am baga a sheachnadh gus nach tèid a mhilleadh aig àm còmhdhail no cleachdadh.
Cùm ann an àrainneachd fionnar, tioram le beatha sgeilp de 12 mìosan.