FV9400
Herchy
| Framboð: | |
|---|---|
| Magn: | |
Atriði |
Vísar |
||||||
Einkunnir |
FV9430 |
FV9440 |
FV9450 |
FV9460 |
FV9470 |
FV9480 |
|
Útlitsprófunaraðferðir |
Mjólkurhvítur hálfgagnsær |
Gulleitur |
|||||
Eðlisþyngd/g/cm3 |
ASTM D792 |
1.38 |
1.41 |
1.42 |
1.43 |
1.45 |
1.47 |
Harka/ströndA |
ASTM D2240 |
28 |
40 |
48 |
60 |
70 |
80 |
Togstyrkur/MPa |
ASTM D412 |
10.2 |
9.5 |
9.5 |
10.2 |
9.9 |
8.1 |
Lenging við brot /% |
ASTM D412 |
485 |
494 |
363 |
296 |
241 |
159 |
Társtyrkur/KN/m |
ASTM D624-B |
18 |
26 |
19 |
22 |
21 |
16 |
Þjöppunarsett (177 ℃ * 22 klst.) |
ASTM D395 |
9 |
8 |
8 |
7 |
8 |
9 |
Seiglu/% |
ASTM D1054 |
41 |
35 |
46 |
40 |
37 |
39 |
* Hitaþol |
Hörkubreyting /shore A |
+2 |
+2 |
+3 |
+2 |
+2 |
+3 |
Togstyrksbreyting, % |
-18 |
-17 |
-21 |
-25 |
-20 |
-19 |
|
Lenging við brotbreytingu, % |
-19 |
-16 |
-18 |
-21 |
-16 |
-15 |
|
Eldsneyti C Hljóðstyrksbreyting/% 23 ℃/72 klst |
ASTM D471 |
+22 |
+19 |
+18 |
+19 |
+19 |
+19 |
Þurrkunarástand |
Bætið við 0,7 hlutum af bis(2+5), eins þrepa gúlkun 170℃×15mín, tveggja þrepa gúlkun: 200℃×4klst. |
||||||
Ráðlagðar aðgerðir:
Mælt er með því að nota 0,6 til 1 hluta af bisdipenta efnafræðilegu efni til vökvunar (2,5-dímetýl-2,5-bis(tert-bútýlperoxý)hexan).
Viðskiptavinir ættu að velja viðeigandi hitastig og tíma til ráðhúss byggt á stærð vörunnar og aðferð við ráðhús.
Vöru umbúðir:
Þessi vara er ekki hættuleg, hún er í staðinn samsett úr pappír, plasti og 10 kílóum í poka, 2 töskur í kassa.
Aldur geymslu:
Þessi vara hefur kalt flæðisgetu, ætti að forðast pokann til að hann skemmist ekki við flutning eða notkun.
Geymist í köldum, þurru umhverfi með 12 mánaða geymsluþol.