Tel: +86 15221953351 E-mail hmanga zawhfiah theih a ni. info@herchyrubber.com
Please Choose Your Language
PRODUCTS THIL THAWN THAWN THIL THIL THIL THIL THIL THIL THIL THIL THIL THAWN

loading a ni

Share to:
facebook ah in share theih a ni
twitter hmanga share theih a ni
line insem theihna button a ni
wechat hmanga insem theihna button a ni
linkedin a insem theihna tur a ni
pinterest hmanga insem theihna button
whatsapp a insem theihna tur a ni
sharethih hi share theih a ni

Fluorosilicone Rubber FV9400 hmanga siam a ni

He product hi base glue atan fluorosilicone elastomer leh filler leh additive hrang hrang homogeneous mixture a ni.
Chakna leh resilience sang tak a nei a ni.
Oil resistance tha tak, solvent resistance tha tak leh temperature sang leh hniam resistance tha tak a ni.
  • FV9400 a ni

  • Herchy a ni

A awm theihna:
A zat:


Thil

Indicators te pawh a awm

Grade hrang hrang a awm

FV9430 a ni

FV9440 a ni

FV9450 a ni

FV9460 a ni

FV9470 a ni

FV9480 a ni

A lan dan
Test dan tur

Milky white translucent a ni

Yellowish a ni

Gravity bik/ g/cm a ni3

ASTM D792 a ni

1.38

1.41

1.42

1.43

1.45

1.47

Hardness/shoreA tih a ni

ASTM D2240 a ni

28

40

48

60

70

80

Tensile chakna/MPa

ASTM D412 a ni

10.2

9.5

9.5

10.2

9.9

8.1

Elongation At Break /% a ni.

ASTM D412 a ni

485

494

363

296

241

159

Mittui chakna/KN/m

ASTM D624-B a ni

18

26

19

22

21

16

A rilru a buai em em a, a rilru a hah em em bawk a. 177°C*22h)

ASTM D395 a ni

9

8

8

7

8

9

Inpawtfan/%

ASTM D1054 a ni

41

35

46

40

37

39

*Heat Resistance
225°C×72h a ni

Harsatna inthlak /shore A

+2

+2

+3

+2

+2

+3

Tensile chakna inthlak danglamna, % .

-18

-17

-21

-25

-20

-19

Break inthlak danglamnaah elongation, % .

-19

-16

-18

-21

-16

-15

Fuel C. a ni

Volume inthlak danglamna/%

23°C/72h a ni

ASTM D471 a ni

+22 a ni

+19 a ni

+18 a ni

+19 a ni

+19 a ni

+19 a ni

Curing Condition a ni

Bis(2+5) hmun 0.7 dah la, stage khat vulcanisation 170°C×15min, stage hnih vulcanisation: 200°C×4h.

Thil tih tur rawtna: 1.1.


Vulcanization atan bisdipenta chemical agent (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane) hmun 0.6 atanga 1 vel hman a rawt a ni.


Customer te chuan an thil siam lian leh te, an tihdam dan a zirin temperature leh hun remchang ber an thlang tur a ni.


Product packaging hrang hrang: 1.1.


He thil hi a hlauhawm lo a, chu ai chuan cardstock, plastic, leh bag khatah kilogram 10, box khatah bag 2 atanga siam a ni.


A dahna kum: 1.1.


He product hian cold flow capacity a nei a, bag hi a phurh chhuah emaw hman lai emaw a chhiat loh nan pumpelh tur a ni.


Thla 12 chhung a awm theihna tur hmun lum leh vawt takah dah tur a ni.


Hma chiah: 
Dawtchiah: 

QUICK LINKS A AWM VE ANG

CONTACT THIL AWM DAN

Add: No.33, Lane 159, Taiye kawngpui, Fengxian District, Shanghai-a awm a ni
Tel / WhatsApp / Skype: +86 15221953351 ah zawhfiah theih a ni
E-mail hmangin:  info@herchyrubber.com
A rilru a hah   lutuk chuan a rilru   2023 a buai em em a. Shanghai Herchy Rubber Co., Ltd. Sitemap a ni |   Thuruk humhalh dan tur | Support By Leadong a ni.