A cikin masana'antar roba, ƙarfin juriya na ƙarshe shine ainihin kayan inji. Wannan siga na gwaji yana auna ƙarfin ƙarshe na mahaɗin roba mara kyau. Ko da samfurin roba ba a taɓa kusantar da ƙarfin ƙarfinsa na ƙarshe ba, yawancin masu amfani da samfuran robar har yanzu suna ɗaukarsa a matsayin muhimmiyar alama ta gabaɗayan ingancin fili. Ƙarfin juzu'i don haka ƙayyadaddun bayanai ne na gaba ɗaya, kuma kodayake ƙarshen amfani da takamaiman samfur ba shi da alaƙa da shi, masu ƙira galibi dole ne su fita hanyarsu don saduwa da shi.
1. Gabaɗaya ka'idoji
Domin samun ƙarfi mafi girma, yakamata mutum ya fara farawa da elastomers inda ƙwaƙƙwaran ƙira zai iya faruwa, misali NR, CR, IR, HNBR.
2. Na halitta roba NR
Adhesives dangane da roba na halitta yawanci suna da ƙarfi mafi girma fiye da adhesives na neoprene. Daga cikin nau'o'i daban-daban na roba na halitta, No. 1 fim din fume yana da mafi girman ƙarfin ƙarfi. An ba da rahoton cewa, aƙalla a cikin yanayin abubuwan da aka cika baƙar fata na carbon, Fim ɗin Fume na 3 yana ba da mafi kyawun ƙarfin ƙarfi fiye da fim ɗin fume No. Don mahadi na roba na halitta, ana amfani da kayan filastik (plastisol) irin su biphenyl amidothiophenol ko pentachlorothiophenol (PCTP), yayin da suke rage ƙarfi na fili.
3. Chloroprene CR
Chloroprene (CR) shine robar lu'ulu'u wanda ke haifar da nau'in lu'u-lu'u wanda ke ba da ƙarfi mai ƙarfi idan babu masu cikawa. A gaskiya ma, ana iya ƙara ƙarfin ƙarfi a wasu lokuta ta hanyar rage adadin filler. Maɗaukakin ma'auni na kwayoyin halitta na CR yana ba da ƙarfi mafi girma.
4. Nitrile roba NBR
NBR tare da babban abun ciki na acrylonitrile (ACN) yana ba da ƙarfi mafi girma. NBR tare da kunkuntar rarraba nauyin kwayoyin halitta yana ba da ƙarfi mafi girma.
5. Tasirin nauyin kwayoyin halitta
Ta hanyar ingantawa, amfani da NBRs tare da babban danko na meniscus da babban nauyin kwayoyin halitta yana ba da ƙarfi mafi girma.
6. Carboxylated elastomers
Yi la'akari da maye gurbin NBR mara karbuwa tare da XNBR na carboxylated da HNBR maras nauyi tare da carboxylated XHNBR don inganta ƙarfin juzu'i na fili.
Carboxylated NBR tare da daidaitaccen adadin zinc oxide yana ba da ƙarfi mafi girma fiye da NBR na al'ada.
7. EPDM
Amfani da Semi-crystalline EPDM (babban abun ciki na ethylene) yana ba da ƙarfi mafi girma.
8. Reactive EPDM
Maye gurbin EPDM wanda ba a canza shi ba tare da 2% (jama'a mai yawa) maleic anhydride modified EPDM a cikin haɗuwa tare da NR yana ƙara ƙarfin juzu'i na mahaɗan NR/EPDM.
9. Gishiri
Gel ɗin roba irin su SBR gabaɗaya sun ƙunshi masu ƙarfafawa. Duk da haka, lokacin da ake hada mahadi na SBR a yanayin zafi sama da 163 ° C, ana iya samar da gels maras kyau (waɗanda za a iya haɗa su) da kuma gels (waɗanda ba za a iya haɗa su ba kuma ba su iya narkewa a cikin wasu kaushi). Duk nau'ikan gel guda biyu suna rage ƙarfin ƙarfi na fili. Sabili da haka, dole ne a kula da yanayin zafin jiki na SBR tare da kulawa.
10. Vulcanisation
Muhimmiyar hanya don samun ƙarfin ƙarfi mai ƙarfi shine haɓaka ƙimar haɗin giciye, guje wa ƙarancin sulphurisation, bayan-vulcanisation da guje wa ƙumburi na roba yayin vulcanisation saboda rashin isasshen matsi ko amfani da abubuwan da ba su da ƙarfi.
11. Matsawa-digon vulcanisation
Don samfuran vulcanised a cikin autoclaves, samuwar blisters da sakamakon raguwar ƙarfin ƙarfi ana iya gujewa ta hanyar rage matsa lamba a hankali har zuwa ƙarshen vulcanisation, wannan ana kiransa 'matsayi drop vulcanisation'.
12. Lokacin vulcanisation da zafin jiki
Dogayen lokutan vulcanisation a ƙananan yanayin zafi yana haifar da samuwar hanyoyin haɗin yanar gizo na sulfur mai yawa, mafi girman sulfur crosslink density kuma saboda haka mafi girman ƙarfi.
13. Ana iya inganta ƙarfin ƙarfin ƙarfi ta hanyar dabarun haɗakarwa mafi kyau don haɓaka tarwatsawar abubuwan ƙarfafawa kamar baƙar fata carbon, yayin da guje wa haɗuwa da ƙazanta ko manyan abubuwan da ba a tarwatsa su ba.
14. Fillers
Don masu cikawa irin su carbon baƙar fata ko silica, zaɓin ƙaramin girman barbashi tare da ƙayyadaddun yanki na musamman na iya zama tasiri a haɓaka ƙarfin ƙarfi. Ya kamata a guje wa abubuwan da ba a ƙarfafawa ko cikawa kamar yumbu, calcium carbonate, talc, yashi quartz, da sauransu.
15. Carbon baki
Don tabbatar da cewa baƙar fata na carbon yana tarwatsewa da kyau, ya kamata a ƙara cika shi zuwa mafi kyawun matakin don haɓaka ƙarfin ƙarfi. Baƙar fata na carbon tare da ƙaramin ƙaramar ɓangarorin zai sami mafi ƙarancin adadin cikawa. Ƙara ƙayyadaddun yanki na baƙar fata na carbon da inganta tarwatsawar baƙar fata ta carbon ta hanyar ƙaddamar da sake zagayowar haɗuwa zai iya inganta ƙarfin ƙarfin roba.
16. White carbon baki
Yin amfani da silica da aka haɗe tare da wani yanki na musamman na musamman zai iya inganta ingantaccen ƙarfin fili na fili.
17. Filastik
Yakamata a guji masu yin filastik idan ana son ƙarfin ƙarfi mai ƙarfi.
18. Lokacin vulcanising NBR mahadi, al'ada vulcanisation ne mafi wuya a tarwatsa ko'ina, sabili da haka, sulfur bi da tare da magnesium carbonate zai tarwatsa mafi kyau a cikin iyakacin duniya mahadi kamar NBR. Idan ba a tarwatse ba da kyaun wakili na vulcanising, ƙarfin taurin zai iya yin tasiri sosai.
19. Multi-sulphur bonded crosslinking cibiyar sadarwa
Tare da tsarin vulcanisation na al'ada, cibiyar sadarwa ta hanyar haɗin gwiwa ta mamaye abubuwan haɗin polysulphide; tare da EV, cibiyar sadarwa ta crosslinking tana mamaye ta hanyar haɗin sulphide guda ɗaya da biyu, wanda ya haifar da ƙarfin ƙarfi mafi girma.
20. Ionic crosslinking cibiyoyin sadarwa
Abubuwan haɗin giciye na Ionic suna da ƙarfin juzu'i mafi girma saboda wuraren da aka haɗa su na iya zamewa kuma don haka suna motsawa ba tare da tsagewa ba.
21. Danniya crystallisation
Haɗuwa da roba na halitta da neoprene wanda ke dauke da lu'ulu'u na damuwa a cikin manne zai taimaka wajen ƙara ƙarfin ƙarfi.