GA-2033 Silicone rɔba (LSR) a ɔde ne ho hyɛ mu .

Application: Ɛfata sɛ wɔyɛ auto afã horow, plug, ne nea ɛkeka ho.
Nneɛma atitiriw: ahoɔden a ɛkorɔn, ngo pa a ɛma mogya tu.
  • GA-2033 na ɛwɔ hɔ.

  • Herchy .

Nneɛma a ɛwɔ hɔ:
Dodoɔ:

Sɔhwɛ: A/B Nkyɛmu yɛ 1 :1, 130°C x 5min x 15MPa .

Product parameters .
Adwadeɛ GA-2033 na ɛwɔ hɔ.
GA-2043 na ɛwɔ hɔ. GA-2053 na ɛwɔ hɔ. GA-2045 na ɛwɔ hɔ.
Mmaeɛ Translucent .
Nneɛma a ɛyɛ den(pa.s) .
2000 3000 4000 3500
Hardness (Shorea) . 30 40 50
40
density(g/cm3) . 1.10 1.12 1.14 1.13
Ahoɔden a ɛyɛ den (MPa) . 6.5
8.0
9.5
7.5
Elongation(%) . 650 550 500 550
Ahoɔden a ɛtetew (kn/m) . 13 20 27
21
LinearSHRINKAGE(%) . 1.8 1.8 1.8 1.8
Nneɛma a wɔde hyɛ mu 175 x 22h (%) . -
-
-
20










Dada: 
Deɛ ɛdi hɔ: 

Links a ɛyɛ ntɛm .

Yɛn nneɛma .

Nsɛm a wɔde di nkitaho .

Fa ka ho: No.33, Lane 159, Taiye kwan so, Fengxian Mantam, Shanghai .
Tel / WhatsApp / Skype: +8615221953351 .
Nsɛm a ɛfa ho     2025 Shanghai Herchy Rubber Co., Ltd. SiteMap . |   Nsɛm a Wɔde Sie Ho Nsɛm | Mmoa a wɔde ma denam . Leang ..