FV9700
I-Herchy
| Ukutholakala: | |
|---|---|
| Ubuningi: | |
Into |
Izinkomba |
||
Inombolo yomkhiqizo |
I-NFS9760 |
I-NFS9770 |
|
Ukubukeka Izindlela Zokuhlola |
Indawo ekhanyayo, ebushelelezi, Akukho ukungcola |
||
I-Gravity ethize/g/cm3 |
I-ASTM D792 |
1.44 |
1.48 |
Ukuqina/uguA |
I-ASTM D2240 |
60 |
70 |
Amandla Okuqina/MPa |
I-ASTM D412 |
10.5 |
10.1 |
Ukwelula Ngekhefu /% |
I-ASTM D412 |
207 |
201 |
Amandla Ezinyembezi/KN/m |
I-ASTM D624-B |
18 |
17 |
Isethi Yokucindezela (177℃*22h) |
Ukuhluka kokuqina/A |
+4 |
+5 |
Izinga lokushintsha kwamandla e-tensile/% |
-27 |
-24 |
|
Izinga lokushintsha kobude/% |
-26 |
-23 |
|
I-Fuel C Ukushintsha Kwevolumu/% 23℃/72h |
I-ASTM D471 |
21 |
20 |
I-IRM903 |
I-ASTM D471 |
4.5 |
4 |
I-nitric acid/sulfuric acid/hydrochloric acid solution exubile PH<1 100℃×120h |
|||
Ukumelana ne-Acid |
I-ASTM D471 |
0.3 |
0.3 |
3% isixazululo sodium hydroxide 60 ℃×72h |
|||
Ukumelana ne-alkali |
I-ASTM D471 |
0.4 |
0.3 |
Isimo Sokwelapha |
0.8 izingxenye ze-bisditetra, i-vulcanisation yesiteji esisodwa 120℃×15min, i-vulcanisation yezigaba ezimbili: 200℃×4h |
||
Izenzo ezinconyiwe:
Kuphakanyiswa ukuthi kusetshenziswe izingxenye ezingu-0.4-0.7 ze-bisdisulfide (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane).
Amakhasimende kufanele akhethe izinga lokushisa elifanele kakhulu nesikhathi sokwelapha ngokusekelwe kusayizi womkhiqizo kanye nendlela yokwelapha.
Ukupakishwa komkhiqizo:
Lo mkhiqizo awuyona ingozi, kunalokho wakhiwe nge-cardstock, ipulasitiki, namakhilogremu ayi-10 isikhwama ngasinye, izikhwama ezi-2 ibhokisi ngalinye.
Iminyaka yokugcina:
Lo mkhiqizo unomthamo wokugeleza okubandayo, isikhwama kufanele sigwenywe ukuze singalimazi ngesikhathi sokuthutha noma ukusetshenziswa.
Gcina endaweni epholile, eyomile eneshalofu impilo yezinyanga eziyi-12.