FV9700
Herchi
| Mavjudligi: | |
|---|---|
| Miqdori: | |
Element |
Ko'rsatkichlar |
||
Ishlab chiqarish raqami |
NFS9760 |
NFS9770 |
|
Tashqi ko'rinish Sinov usullari |
Shaffof, silliq sirt, Hech qanday iflosliklar yo'q |
||
O'ziga xos tortishish / g / sm3 |
ASTM D792 |
1.44 |
1.48 |
Qattiqlik / qirg'oqA |
ASTM D2240 |
60 |
70 |
Kuchlanish kuchi/MPa |
ASTM D412 |
10.5 |
10.1 |
Uzilishdagi cho'zilish /% |
ASTM D412 |
207 |
201 |
Yirtilish kuchi/KN/m |
ASTM D624-B |
18 |
17 |
Siqish to'plami (177 ℃ * 22 soat) |
Qattiqlik o'zgarishi / A |
+4 |
+5 |
Kuchlanish kuchining o'zgarish darajasi /% |
-27 |
-24 |
|
Cho'zilishning o'zgarish darajasi /% |
-26 |
-23 |
|
Yoqilg'i C Ovoz balandligi/% 23℃/72 soat |
ASTM D471 |
21 |
20 |
IRM903 |
ASTM D471 |
4.5 |
4 |
Nitrat kislota/sulfat kislota/xlorid kislota aralash eritmasi PH<1 100℃×120h |
|||
Kislota qarshiligi |
ASTM D471 |
0.3 |
0.3 |
3% natriy gidroksid eritmasi 60 ℃ × 72 soat |
|||
Ishqor qarshiligi |
ASTM D471 |
0.4 |
0.3 |
Qattiqlashuv holati |
Bisditetraning 0,8 qismi, bir bosqichli vulkanizatsiya 120 ℃ × 15 min, ikki bosqichli vulkanizatsiya: 200 ℃ × 4 soat |
||
Tavsiya etilgan harakatlar:
0,4-0,7 qism bisdisulfid (2,5-dimetil-2,5-bis (tert-butilperoksi) geksan) dan foydalanish tavsiya etiladi.
Iste'molchilar mahsulotning o'lchami va quritish usulidan kelib chiqib, eng mos harorat va quritish vaqtini tanlashlari kerak.
Mahsulot qadoqlash:
Ushbu mahsulot xavfli emas, uning o'rniga karton, plastmassa va har bir sumka uchun 10 kilogramm, har bir qutiga 2 ta qopdan iborat.
Saqlash muddati:
Ushbu mahsulot sovuq oqim qobiliyatiga ega, tashish yoki foydalanish paytida uni shikastlamaslik uchun sumkadan qochish kerak.
Salqin, quruq muhitda saqlash muddati 12 oy.