Tel: +8615221953351   E-mail: info@herchyrubber.com
PRODUCTS
You are here: Home » Products » Synthesis Rubber » FVMQ Fluorosilicone » FV9700 Fluorosilicone

loading

Share to:
facebook sharing button
twitter sharing button
line sharing button
wechat sharing button
linkedin sharing button
pinterest sharing button
whatsapp sharing button
sharethis sharing button

FV9700 Fluorosilicone

This product is suitable for extrusion moulding of bis-disulfide. It has excellent oil resistance, solvent resistance, acid and alkali resistance.
  • FV9700

  • Herchy

Availability:
Quantity:

Technical indicators



Item

Indicators

Serial number

NFS9760

NFS9770

Appearance

Test Methods

Translucent, smooth surface,

No impurities

Specific Gravity/ g/cm3

ASTM D792

1.44

1.48

Hardness/shoreA

ASTM D2240

60

70

Tensile Strength/MPa

ASTM D412

10.5

10.1

Elongation At Break /%

ASTM D412

207

201

Tear Strength/KN/m

ASTM D624-B

18

17

Compression Set(177℃*22h)

Hardness variation/A

+4

+5

Rate of change of tensile strength/%

-27

-24

Rate of change of elongation/%

-26

-23

Fuel C

Volume Change/%

23℃/72h

ASTM D471

21

20

IRM903
Volumetric rate of change/%
150℃×72h

ASTM D471

4.5

4

Nitric acid/sulfuric acid/hydrochloric acid mixed solution PH<1 100℃×120h

Acid resistance
Volume change rate/%

ASTM D471

0.3

0.3

3% sodium hydroxide solution 60℃×72h

Alkali resistance
Volume change rate/%

ASTM D471

0.4

0.3

Curing Condition

0.8 parts of bisditetra, one-stage vulcanisation 120℃×15min, two-stage vulcanisation: 200℃×4h

Recommended actions:


It's suggested to utilize 0.4-0.7 parts of bisdisulfide (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane).


Customers should choose the most appropriate temperature and time for curing based on the product's size and method of curing.


Product packaging:


This product is not dangerous, it's instead composed of cardstock, plastic, and 10 kilograms per bag, 2 bags per box.


Age of storage:


This product has a cold flow capacity, the bag should be avoided in order to not have it damaged during transportation or utilization.


Keep in a cool, dry environment with a shelf life of 12 months.


Previous: 
Next: 

QUICK LINKS

OUR PRODUCTS

CONTACT INFORMATION

Add: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +8615221953351
Copyright  2023 Shanghai Herchy Rubber Co., Ltd. Sitemap |  Privacy Policy | Support By Leadong.