FVL-7435
Herchy
| Avanoa: | |
|---|---|
| Aofa'i: | |
Aitema |
Metotia Su'ega |
NFS-L-7435 |
Fa'aaliga A |
iloiloga vaaia |
samasama |
Fa'aaliga B |
iloiloga vaaia |
samasama |
Viscosity / Pa.s A (sele fua 10 s -1 ) |
Q/371002WXH028-2016 |
350 |
Viscosity / Pa.s B (sele fua 10 s -1 ) |
Q/371002WXH028-2016 |
300 |
25℃×48h |
||
Gravity Fa'apitoa/g/cm3 |
ASTM D792 |
1.42 |
Ma'a'a/TagafagaA |
ASTM D2240 |
35 |
Malosi Tetele/MPa |
ASTM D412 |
8.1 |
Fa'aumi ile malologa /% |
ASTM D412 |
320 |
Malosi Loimata/KN/m |
ASTM D624-B |
14.5 |
Talitonu/% |
ASTM D1054 |
36 |
Seti fa'amalosi/%(177℃×22h) |
ASTM D395 |
21 |
Suau'u C Suiga Volume /% (25℃×72h) |
ASTM D471 |
24.0 |
Fa'aoga:
NFS-L-7435 paʻu fluorosilicone vai o loʻo faʻapipiʻiina i vaega e lua. A faʻaaogaina, vaega A, B e tusa ai ma le fua faʻatatau o le 1: 1 faʻafefiloi ma le faʻaleagaina o togafitiga, o le vevela o le potu (25 ℃ ± 5 ℃) tuʻuina i le 48h e mafai ona faʻamalolo atoatoa.
afifiina:
Tu'u i totonu o pa'u palasitika, 20kg mo vaega A/B ta'itasi.
Taimi e teu ai:
Teuina i totonu o se siosiomaga malulu ma mago, e le'i tatalaina uluai afifiina taimi teuina mo le sefululua masina.
Fa'aeteetega:
Aloese mai le fa'afeso'ota'i ma fa'aputuga o lo'o i ai le nitrogen, sulfur, phosphorus ma u'amea mamafa, e ono fa'aoso ai le oloa e fa'apala e le'i vela pe leai fo'i vulcanise.