GA-2340
Herchy
| Boteng: | |
|---|---|
| Bongata: | |
Teko: AB karo-karolelano ea 10:1 kapa 1:1, 130'C x 5min x 15Mpa.
| Lihlahisoa tsa lihlahisoa | |||
| Sehlahisoa | GA-2340 |
GA-2341 | |
| Ponahalo | Translucent | ||
| A/Bratio | A:B=10:1 |
A:B=1:1 |
|
| Viscosity(Pa.s) |
50/1 | 75/75 | |
| Ho thatafala (LebopoA) | 38 | 38 | |
| Boima ba 'mele(g/cm3) | 1.08 | 1.08 | |
| Tensile Matla (MPa) | 6.5 |
6.5 |
|
| Elongation(%) | 400 | 400 | |
| Matla a ho lla (kN/m) | 18 | 18 | |
| Linearshrinkage(%) | 2.0 |
2.0 | |