GA-2340
Herchy
| Availability: | |
|---|---|
| Dami: | |
Pagsubok: AB ratio na 10:1 o 1:1, 130'C x 5min x 15Mpa.
| Mga parameter ng produkto | |||
| produkto | GA-2340 |
GA-2341 | |
| Hitsura | Translucent | ||
| A/Bratio | A:B=10:1 |
A:B=1:1 |
|
| Lagkit(Pa.s) |
50/1 | 75/75 | |
| Katigasan (ShoreA) | 38 | 38 | |
| Densidad(g/cm3) | 1.08 | 1.08 | |
| Lakas ng makunat (MPa) | 6.5 |
6.5 |
|
| Pagpahaba(%) | 400 | 400 | |
| Lakas ng luha (kN/m) | 18 | 18 | |
| Linearshrinkage(%) | 2.0 |
2.0 | |