GA-2610
Herchy
| Boteng: | |
|---|---|
| Bongata: | |
Teko: A/B karo-karolelano ea 1 :1, 130°C x 5min x 15MPa
| Lihlahisoa tsa lihlahisoa | |||||||||
| Sehlahisoa | GA-2610 | GA-2620 | GA-2630 | GA-2640 | GA-2650 | GA-2660 | GA-2670 | GA-2680 | |
| Ponahalo | Tse pepeneneng | ||||||||
| Viscosity(Pa.s) |
1500 | 2000 | 2500 | 3000 | 3500 | 4000 |
4000 |
5500 |
|
| Ho thatafala (LebopoA) | 10 | 20 | 30 | 40 | 50 |
60 |
70 |
80 |
|
| Boima ba 'mele(g/cm3) | 1.08 | 1.10 | 1.10 | 1.11 | 1.12 |
1.13 |
1.14 |
1.15 |
|
| Tensile Matla (MPa) | 4.5 |
6.5 |
7.5 |
9.5 |
10.0 |
10.0 |
9.5 |
9.0 |
|
| Elongation(%) | 900 | 880 | 800 | 700 | 550 |
450 |
350 |
350 |
|
| Matla a ho lla (kN/m) | 8 | 12 | 15 | 25 | 35 |
35 |
30 |
30 |
|
| Linearshrinkage(%) | 2.3 | 2.1 | 2.1 | 2.1 | 2.0 |
2.0 |
2.0 |
2.0 |
|
| Phetiso(%) | 90 |
90 | 90 | 90 | 90 | 90 | 90 | 90 | |