GA-2100D
Herchy nga bwe kiri
| Okubeerawo: | |
|---|---|
| Omuwendo: | |
Okugezesebwa: Omugerageranyo gwa A:B ogwa 1:1, 130°C x 5min x 15MPa.
| Ebipimo by’ebintu | |||||||
| Ekyamaguzi | GA-2100D | GA-2105D | GA-2110D | GA-2115D | GA-2120D | GA-2125D | |
| Endabika | Etangalijja | ||||||
| Obuziba(Pa.s) . |
A:1.0 B:1.0 |
A:4.0 B:4.0 |
A:3.0 B:3.0 |
A:3.5 B:3.5 |
A:4.6 B:4.3 |
A:4.5 B:4.5 |
|
| Obukaluba (ShoreA) . | 0 | 5 | 10 | 15 |
20 |
25 |
|
| Obugumu(g/cm3) . | 1.10 |
1.10 |
1.12 |
1.12 | 1.10 |
1.12 |
|
| Amaanyi g’okusika (MPa) . | 0.4 |
2.5 |
3.0 |
4.0 |
6.0 |
6.0 |
|
| Okuwanvuwa(%) . | 500 | 500 | 600 | 550 | 600 |
600 |
|
| Amaanyi g’okukutuka (kN/m) . | 1.5 | 8 | 7 |
8 | 11 |
14 |
|