GA-2610
Herchy .
| Ebiriwo: | |
|---|---|
| Omuwendo: | |
Okugezesa: Omugerageranyo gwa A/B ogwa 1 :1, 130°C x 5min x 15MPa
| Ebipimo by'ebintu . | |||||||||
| Ekyamaguzi | GA-2610 | GA-2620 | GA-2630 | GA-2640 | GA-2650 | GA-2660 | GA-2670 | GA-2680 | |
| Endabika | Okutangaala | ||||||||
| Obuziba(Pa.s) . |
1500 | 2000 | 2500 | 3000 | 3500 | 4000 |
4000 |
5500 |
|
| Obukakanyavu (Shorea) . | 10 | 20 | 30 | 40 | 50 |
60 |
70 |
80 |
|
| Densite(g/cm3) . | 1.08 | 1.10 | 1.10 | 1.11 | 1.12 |
1.13 |
1.14 |
1.15 |
|
| Amaanyi g’okusika (MPA) . | 4.5 |
6.5 |
7.5 |
9.5 |
10.0 |
10.0 |
9.5 |
9.0 |
|
| okuwanvuwa(%) . | 900 | 880 | 800 | 700 | 550 |
450 |
350 |
350 |
|
| Amaanyi g’okukutuka (kn/m) . | 8 | 12 | 15 | 25 | 35 |
35 |
30 |
30 |
|
| Okukendeera kw’ennyiriri(%) . | 2.3 | 2.1 | 2.1 | 2.1 | 2.0 |
2.0 |
2.0 |
2.0 |
|
| Okutambuza(%) . | 90 |
90 | 90 | 90 | 90 | 90 | 90 | 90 | |