Tεst: 1% pan di kכring ejen (50% paste fכ DBPMH insay silikon gכm), 175° x 5min x 15MPa
| Prodakt paramita dɛn | |||||||
| Sɔntin | GA-1023 we dɛn kɔl |
GA-1033 we dɛn kɔl | GA-1043 we dɛn kɔl | GA-1053 we dɛn kɔl | GA-1063 we dɛn kɔl | GA-1073 we dɛn kɔl | GA-1083 we dɛn kɔl |
| Aw a luk | Translucent we de mek pɔsin fil fayn | ||||||
| Wiliamplastisiti |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
| Di hadnɛs (ShoreA) . |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
| Densiti(g/cm3) . | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Tεnsilεrεngth (MPa) . |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
| Elongation(%) we de go bifo. | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
| Di trɛnk we pɔsin kin kray (kN/m) . | 10 |
16 |
20 |
20 |
20 |
20 |
16 |