Test: 1% kurermiddel (50% pasta fan DBPMH yn silikongom), 175 ° x 5min x 15MPa
| Produkt parameters | |||||||
| Produkt | GA-1023 |
GA-1033 | GA-1043 | GA-1053 | GA-1063 | GA-1073 | GA-1083 |
| Ferskining | Trochsichtich | ||||||
| Williamplasticity |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
| Hardheid (ShoreA) |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
| Tichtheid (g/cm3) | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Treksterkte (MPa) |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
| Ferlinging (%) | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
| Tearsterkte (kN/m) | 10 |
16 |
20 |
20 |
20 |
20 |
16 |