GA-10×3
Hercy
| Ketersediaan: | |
|---|---|
| Kuantitas: | |
Pengujian: 1% bahan pengawet (50% pasta DBPMH dalam permen karet silikon), 175° x 5 menit x 15MPa
| Parameter produk | |||||||
| Produk | GA-1023 |
GA-1033 | GA-1043 | GA-1053 | GA-1063 | GA-1073 | GA-1083 |
| Penampilan | Tembus cahaya | ||||||
| Williamplastisitas |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
| Kekerasan (ShoreA) |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
| Massa jenis (g/cm3) | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Kekuatan tarik (MPa) |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
| Pemanjangan(%) | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
| Kekuatan sobek (kN/m) | 10 |
16 |
20 |
20 |
20 |
20 |
16 |