Ga-10 × 3
Hercy
Hatility: | |
---|---|
Qumar: | |
Test: 1% ji Agent Curing (50% Paste of DBPMH li Silicone Gum), 175 ° X 5min X 15mpa
Parametreyên hilberê | |||||||
Mal | GA-1023 |
GA-1033 | GA-1043 | GA-1053 | GA-1063 | GA-1073 | GA-1083 |
Xuyabûnî | Teyz | ||||||
Williamplasticity |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
Hardness (Shorea) |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
Dendik (g / cm3) | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
Tenilestrength (Mpa) |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
Elongation (%) | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
Tearstrength (kn / m) | 10 |
16 |
20 |
20 |
20 |
20 |
16 |
Test: 1% ji Agent Curing (50% Paste of DBPMH li Silicone Gum), 175 ° X 5min X 15mpa
Parametreyên hilberê | |||||||
Mal | GA-1023 |
GA-1033 | GA-1043 | GA-1053 | GA-1063 | GA-1073 | GA-1083 |
Xuyabûnî | Teyz | ||||||
Williamplasticity |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
Hardness (Shorea) |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
Dendik (g / cm3) | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
Tenilestrength (Mpa) |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
Elongation (%) | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
Tearstrength (kn / m) | 10 |
16 |
20 |
20 |
20 |
20 |
16 |