GA-10×3 a ni
Hercy chuan a rawn ti a
| A awm theihna: | |
|---|---|
| A zat: | |
Test: Curing agent 1% (silicone gum-a DBPMH paste 50%), 175° x 5min x 15MPa
| Product Parameters 1000 a ni. | |||||||
| Thilsiam | GA-1023-ah a awm |
GA-1033 ah a awm | GA-1043 ah a awm | GA-1053-ah a awm | GA-1063-ah a awm | GA-1073-ah a awm | GA-1083-ah a awm |
| Landan | Translucent a ni | ||||||
| Williamplasticity . |
100 |
115 |
150 |
205 |
240 |
280 |
310 |
| Harsatna (Shorea) . |
20 |
30 |
40 |
50 |
60 |
70 |
80 |
| Density(g/cm3) a ni. | 1.08 |
1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Tensil chakna (MPa) 1.1. |
6 |
7 |
8 |
9 |
8 |
8 |
7 |
| A sei zawng(%) . | 900 |
750 |
650 |
550 |
450 |
350 |
150 |
| Mittui tlak chakna (kN/m) . | 10 |
16 |
20 |
20 |
20 |
20 |
16 |