| Adzɔnuwo ƒe nɔnɔmetatawo . |
|
| Nu si wowɔ |
GA-2040D ƒe agbalẽa
|
GA-2040D-45 ƒe agbalẽ
|
GA-20400-60 ƒe agbalẽ
|
| Dzedzeme |
Aŋutiɖiɖi si me kɔ/tedzi/dzẽ |
Aŋutiɖiɖi si me kɔ |
Fu |
Nusiwo le ʋeʋẽmA (Pa·s) .
|
250-400 ƒe xexlẽdzesiwo |
70-100 me |
Ƒe 1500-2000 me
|
Nusiwo le ʋeʋẽmB (Pa·s) .
|
250-400 ƒe xexlẽdzesiwo |
70-100 me |
Ƒe 1500-2000 me |
| Sesẽ (Shorea) . |
43-48 me |
37-43 me |
55-60 me |
| Eƒe kpekpeme(g/cm 3) . |
1.11
|
1.11
|
1.15
|
| Tensile ƒe ŋusẽ (MPA) . |
7
|
7.0
|
8.5
|
| Elongation(%) . |
500 |
450 |
550 |
| Aɖatsiŋusẽ (kn/m) . |
22
|
22
|
35
|
| Dielectric ɣesiaɣi le 100HZ |
3.03 |
2.95
|
3.3 |
| Nusiwo kakana le 100HZ |
0.0016 |
0.0017 |
0.004 |
| Tsitretsitsi ɖe elektrikŋusẽ ƒe sisi kple dzesidede ŋu |
1A3.5 |
1A4.5 |
1A3.5 |
| Dielektrikŋusẽ ƒe Ŋusẽ (kV/mm) . |
24 .3
|
20.5
|
22
|
| Agbɔsɔsɔme ƒe Tsitretsitsi (Ω·cm) . |
1.0 *1015 |
1.0 *1015 |
1.0 *1015 |
| Dzo ƒe klass |
FV-0-0 |
FV-0-0 |
FV-0-0 |