| Tipharamitha ta Xiendliwa . |
|
| Ximakiwa |
GA-2040D
|
GA-2040D-45
|
GA-20400-60
|
| Xivumbeko |
Grey yo vonikela/kamela/yo tshwuka |
Muhlovo wa grey wo vonikela |
Mpunga |
Ku tsindziyelaA (Pa·s) .
|
250-400 |
70-100 |
1500-2000
|
Ku tsindziyelaB (Pa·s) .
|
250-400 |
70-100 |
1500-2000 |
| Ku nonon'hwa (Shorea) . |
43-48 |
37-43 |
55-60 |
| Ku tsindziyela(g/cm 3) . |
1.11
|
1.11
|
1.15
|
| Matimba ya ku tsana (MPA) . |
7
|
7.0
|
8.5
|
| Ku leha(%) . |
500 |
450 |
550 |
| Matimba ya ku handzuka (KN/M) . |
22
|
22
|
35
|
| Dielectric constant eka 100HZ |
3.03 |
2.95
|
3.3 |
| Xiphemu xa ku hangalaka eka100HZ |
0.0016 |
0.0017 |
0.004 |
| Ku lwisana na ku khuluka ka gezi na ku fungha |
1A3.5 |
1A4.5 |
1A3.5 |
| Matimba ya Dielectric (kV/mm) . |
24 .3
|
20.5
|
22
|
| Vutshila bya Vholumo (Ω·cm) . |
1.0 *1015 |
1.0 *1015 |
1.0 *1015 |
| Tlilasi ya malangavi |
FV-0 |
FV-0 |
FV-0 |