Tijaabada: saamiga AB ee 1: 1, 130°C x 5min x 15MPa
| Xuduudaha alaabta |
|
| Alaabta |
GA-2040D
|
GA-2040D-45
|
GA-20400-60
|
| Muuqashada |
Cawlan fudud/geel/cas |
Cawlan khafiif ah |
Cawlan |
ViscosityA (Pa·s)
|
250-400 |
70-100 |
1500-2000
|
ViscosityB (Pa·s)
|
250-400 |
70-100 |
1500-2000 |
| Adag ( ShoreA) |
43-48 |
37-43 |
55-60 |
| Cufnaanta (g/cm 3) |
1.11
|
1.11
|
1.15
|
| Xoog xajin (MPa) |
7
|
7.0
|
8.5
|
| Dheeraynta(%) |
500 |
450 |
550 |
| Xoogga jeexjeexa (kN/m) |
22
|
22
|
35
|
| Dielectric joogto ah oo ah 100HZ |
3.03 |
2.95
|
3.3 |
| Qodobka kala daadsanaanta 100HZ |
0.0016 |
0.0017 |
0.004 |
| U adkaysiga daadinta korantada iyo calaamadaynta |
1A3.5 |
1A4.5 |
1A3.5 |
| Xoogga Korontada (kV/mm) |
24.3
|
20.5
|
22
|
| Cadaadiska Mugga (Ω·cm) |
1.0 *1015 |
1.0 *1015 |
1.0 *1015 |
| Heerka ololka |
FV-0 |
FV-0 |
FV-0 |