| Ba paramètres ya produit | |||||||||
| Eloko | GA-2610 | GA-2620 oyo ezali na kati | GA-2630 oyo ezali na kati | GA-2640 oyo ezali na kati | GA-2650 oyo ezali na kati | GA-2660 na nzela ya mokanda | GA-2670 | GA-2680 | |
| Komonana | Ezomonana na kati | ||||||||
| Viscosité(Pa.s) ya . |
1500 | 2000 | 2500 | 3000 | 3500 | 4000 |
4000 |
5500 |
|
| Bokasi ya makasi (ShoreA) . | 10 | 20 | 30 | 40 | 50 |
60 |
70 |
80 |
|
| Densité(g/cm3) Ezali na ba . | 1.08 | 1.10 | 1.10 | 1.11 | 1.12 |
1.13 |
1.14 |
1.15 |
|
| Bokasi ya kokangama (MPa) . | 4.5 |
6.5 |
7.5 |
9.5 |
10.0 |
10.0 |
9.5 |
9.0 |
|
| Elongation(%) ya . | 900 | 880 | 800 | 700 | 550 |
450 |
350 |
350 |
|
| Bokasi ya kopasola (kN/m) . | 8 | 12 | 15 | 25 | 35 |
35 |
30 |
30 |
|
| Bokiti ya linéaire(%) . | 2.3 | 2.1 | 2.1 | 2.1 | 2.0 |
2.0 |
2.0 |
2.0 |
|
| Bopanzi sango(%) . | 90 |
90 | 90 | 90 | 90 | 90 | 90 | 90 | |