Test: Curing agent 1% (silicone gum-a DBPMH paste 50%), 175心5minx 15MPa.
| Product Parameters 1000 a ni. | |||||
| Thilsiam | GA-9931 a ni | GA-9941 hmanga tih a ni | GA-9951 a ni | GA-9961 a ni | GA-9971 hmanga tih a ni |
| Landan | Translucent a ni | ||||
| Williamplasticity . | 120 | 130 | 150 | 170 | 180 |
| Harsatna (Shorea) . | 30 | 40 | 50 | 60 | 70 |
| Density(g/cm3) a ni. | 1.1 | 1.11 | 1.12 | 1.14 | 1.16 |
| Tensile chakna (MPA) . | 6 | 6 | 6 | 6 | 6.5 |
| A sei zawng(%) . | 800 | 500 | 250 | 200 | 150 |
| Mittui tlak chakna (kN/m) . | 15 | 15 | 15 | 15 | 15 |
| 175'C x22h Compression Set(%) a ni. | 15 | 10 | 8 | 8 | 10 |