GA-9331 ah a awm
Herchy a ni
| A awm theihna: | |
|---|---|
| A zat: | |
Test: Curing agent 1% (silicone gum-a DBPMH paste 50%), 175° x5minx15MPa
| Product Parameters 1000 a ni. | |||||
| Thilsiam | GA-9331 ah a awm |
GA-9341 a ni | GA-9351 ah a awm | GA-9361 ah a awm | GA-9371 ah a awm |
| Landan | MilkyWhite a ni | ||||
| Williamplasticity . |
120 |
150 |
180 |
210 |
240 |
| Harsatna (Shorea) . |
30 |
40 |
50 |
60 |
70 |
| Density(g/cm3) a ni. | 1.12 |
1.14 |
1.17 |
1.20 |
1.21 |
| Tensile chakna (MPA) . |
8.0 |
8.5 |
8.5 |
8.0 |
7.0 |
| A sei zawng(%) . | 800 |
600 |
500 |
400 |
300 |
| Tear chakna (kn/m) . | 18 |
18 |
20 |
20 |
20 |