GA-91X3-ah a awm
Herchy a ni
| A awm theihna: | |
|---|---|
| A zat: | |
Test: Curing agent 1% (silicone gum-a DBPMH paste 50%), 175° x5minx15MPa
| Product Parameters 1000 a ni. | |||||
| Thilsiam | GA-9133-ah a awm |
GA-9143 hmanga tih a ni | GA-9153 ah a awm | GA-9163 ah a awm | GA-9173 ah a awm |
| Landan | Translucent 1000 a ni. | ||||
| Harsatna (Shorea) . |
30 |
40 |
50 |
60 |
70 |
| Density(g/cm3) a ni. | 1.08 |
1.12 |
1.14 |
1.16 |
1.18 |
| Tensile chakna (MPA) . |
3.5 |
4.0 |
5.0 |
6.0 |
6.0 |
| A sei zawng(%) . | 550 |
550 |
450 |
350 |
200 |
| Tear chakna (kn/m) . | 10 |
14 |
16 |
16 |
16 |
| Lei chunglam atanga a invenna (Ω) . |
108--109 |
||||