Mogala: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
DIHLAHISWA
O mo: Gae » Ditšweletšwa » Rabara ya tswako . » Silicone ya VMQ » GA-99X1 Tlaase Kgatelelo Set Silicone Rabara (HCR)

Go Laetša .

Abelana go: .
Konopo ya go abelana ya Facebook .
Konopo ya go abelana ya Twitter .
Konopo ya go abelana ka mola .
WeChat go abelana konope .
Konopo ya go abelana ya LinkedIn .
Pinterest Konopo ya go abelana .
WhatsApp go abelana konope .
AbelanaThis konopo ya go abelana .

GA-99x1 tlase compression sete silicone rabara (HCR) .

Kopo: loketseng bakeng sa tlhahiso ea tiiso lesale, cots, likarolo koloi le otherproducts.
Senotlolo tšobotsi: phahameng manyela, tlaase compression sete, bao e seng chefo tasteless HSE, feta theauthentication ya RoHS, REACH le FDA.
  • GA - 9 9 X 1

  • Herchy .

Go hwetšagala:
Palo: .

Teko: 1% ya moemedi wa go fodiša (50% ya peista ya DBPMH ka gare ga mare a silicone), 175心5minx 15MPa.


Ditekanyetšo tša Setšweletšwa .
Setšweletšwa GA-9931 ya go swana le GA - 9 9 41 GA-9951 ya go swana le GA - 9 9 61 GA - 9 9 71
Ponagalo Translucent .
Williamplasticity . 120 130 150 170 180
Go thatafala (Sorea) . 30 40 50 60 70
Kitlano (G / CM3) . 1.1 1.11 1.12 1.14 1.16
Matla a go goga (MPA) . 6 6 6 6 6.5
go telefa (%) . 800 500 250 200 150
Matla a Meokgo (KN/M) . 15 15 15 15 15
175 'C x22h Sete ya Kgatelelo (%) 15 10 8 8 10


Peleng: 
Latelago: 

Dikgokagano tša ka pela .

Ditšweletšwa tša rena .

TSHEDIMOŠO YA KGOKAGANO

Add: No.33, Lane 159, Tsela ya Taiye, Setereke sa Fengxian, Shanghai
Mogala / WhatsApp / Skype: +86 15221953351
E-mail: .  info@herchyrubber.com
Tokelo ya ngwalollo e ileditšwe     2023 Shanghai Herchy Rabara Co., Ltd. Mmapa wa Sebaka |   Pholisi ya Sephiri | Thekgo Ka Leadong ..