Simba rakasvibira rine huremu hukuru kana zvasvika pakudzivirira kuputika panguva yechipiri yekugadzirwa kwetai kana kana zvasvika pakudzivirira kudonha kweiyo yakaoma extruded profile nekuda kwesimba rinokwevera.
1. Pesvedzero yeuremu hwemamorekuru
Kazhinji kutaura, kukwirisa huremu hwema molecular ye elastomer yakasarudzwa, ndipo pakakwirira simba reGreen. Panyaya yeSBR, huwandu hwepamusoro huremu huremu hunoshandiswa, asi huremu hwakanyanya huremu hunogona kutungamirira kune mamwe matambudziko ekugadzirisa.
2. Strain-induced crystallization
Manamira ane strain-induced crystallization anowanzo kuve nepamusoro peGreen simba.
3. Rabha yakasikwa
Natural rabha ine yakakwirira Green simba. NR ine yakakwira Green simba nekuda kwekuti inopenya kana yakatambanudzwa. Masikirwo eglue ane huwandu hwepamusoro hwemafuta asidhi ester mapoka ane simba reGreen rakakwirira nekuda kwehukuru hwekristaro mukukakavadzana, kazhinji neine mashoma emukati emafuta acid ester mapoka angangoita 2.8 mmol/kg.
4. Vhara mapolima
Kuvapo kwezvishoma zvidiki zve block styrene mune zvisina tsarukano copolymer SBR adhesives inogona kupa iyo inonamira simba rakanaka reGreen.
5. Semi-crystalline EPDM
Sarudzo ye semi-crystalline EPDM ine yakakwira ethylene yemukati inogona kupa iyo inonamira yakanaka Green simba pakudziya kwekamuri.
6. Metallocene-catalyzed EPDM
Iyo imwechete inoshanda centre limited geometry metallocene catalyst tekinoroji inogonesa kugadzirwa kweyakakwira ethylene yemukati EPDM pamwero mukuru. Iyi EPDM ine yakakwira ethylene yemukati ine yakakwira Green's simba. Neiyi tekinoroji iyo ethylene yemukati inogona kudzorwa uye iyo Green's simba reEPDM rinogona kuwedzera kuwedzera.
7. Molecular weight distribution
NBR makomisheni ane nhete yemamorekuru kugoverwa ane yakakwira Green's simba.
8. CR
Simba reGreen Green rinogona kuwanikwa nekusarudza nekukurumidza crystallising neoprene. Kuwedzerwa kweSBR ine yakakwira styrene zvemukati kuCR inogona kuvandudza simba reGreen.
Pakati pemhando dzakasiyana-siyana dze neoprene, Type T neoprene ine yakanyanya kuramba kudonha uye deformation, kureva simba reGreen repamusoro, rinoteverwa neType W. Type G neoprene ine simba rakaipisisa reGreen.
9. Polytetrafluoroethylene
Teflon additives inovandudza simba reGreen rekunamatira.
10. Carbon dema
Carbon dema ine nzvimbo yakakwirira uye chimiro chepamusoro inovandudza simba reGreen rerabha. n326 inowanzoshandiswa mumatairi akavhara nokuti inopa rabha simba reGreen rakakwirira apo ichichengetedza viscosity yakaderera zvakakwana kuti waya ipinde.
Nokuda kwesimba reGreen rakanaka, kabhoni dema ine chimiro chepamusoro uye nzvimbo yakaderera yepamusoro inofanira kushandiswa. Izvi zvinodaro nekuti yakaderera nzvimbo kabhoni nhema inobvumira vhoriyamu yekuzadza yakakwirira, iyo inozowedzera simba reGreen.
11. Kusanganisa
Mukuita kusanganisa, kana elastomer yanyanya-plastiki, simba reGreen remukomboni richadzikiswa.