GA-9540
Herchy
| Avanoa: | |
|---|---|
| Aofaʻi: | |
Suʻega: 1% o le vailaʻau faʻamalolo (50% faʻapipiʻi o le DBPMH i le silicone gum), 175 ° C x 5min x 15MPa.
| Fa'atauga o oloa | ||||
| Oloa | GA-9540 |
GA-9550 | GA-9560 | GA-9570 |
| Fa'aaliga | Translucent | |||
| William palasiti |
155 |
200 |
220 |
250 |
| Malosi (ShoreA) |
40 |
50 |
60 |
70 |
| Malosi (g/cm3) | 1.14 |
1.17 |
1.19 |
1.20 |
| Malosi fa'amalosi (MPa) |
8.0 |
9.0 |
10.0 |
11.0 |
| Fa'atele(%) | 600 |
500 |
450 |
300 |
| Malosi o loimata (kN/m) | 14 |
25 |
25 |
25 |