GA-60X1A hmanga siam a ni
Herchy a ni
| A awm theihna: | |
|---|---|
| A zat: | |
GA-60X1A Silicone Rubber (250 Leh 300 OC) (HCR) hmanga siam a ni.
A hman dan: auto parts, heat-resistant cots, heat-resistantseals leh thil dang siamna atan a tha.
Thil pawimawh tak tak: heat resistance tha leh mechanical strength, RoHS, REACH, leh FDA te authentication pass.
Test: Curing agent 1% (silicone gum-a DBPMH paste 50%),175°C x 5min x 15MPa。
| 250 degree Product parameters a ni | |||||
| Thilsiam | GA-6041A hmanga tih a ni | GA-6051A hmanga tih a ni | GA-6061A hmanga tih a ni | GA-6071A hmanga tih a ni | |
| Landan | Translucent a ni | ||||
| Williamplasticity . | 150 | 200 | 240 | 240 | |
| Harsatna (Shorea) . | 40 | 50 | 60 | 70 | |
| Density(g/cm3) a ni. | 1.14 | 1.16 | 1.18 | 1.2 | |
| Tensile chakna (MPA) . | 8.5 | 9 | 9.5 | 9 | |
| A sei zawng(%) . | 700 | 600 | 500 | 400 | |
| Mittui tlak chakna (kN/m) . | 15 | 20 | 25 | 25 | |
| boruak a upa 250°C x70H a ni | Hardness a ni | 45 | 54 | 64 | 75 |
| Tension chakna a ni | 6.2 | 7.3 | 7.5 | 6.5 | |
| Elongation tih hi a ni | 380.0 | 300.0 | 280.0 | 200.0 | |