Okugezesa: 1.3% eky’ekirungo ekiwonya (50% ekikuta kya DCBP mu silicone gum),130°C x 5min x 15MPa
| Ebipimo by'ebintu . | |||||
| Ekyamaguzi | GA-3240J |
GA-3250J | GA-3260J | GA-3270J | GA-3280J |
| Endabika | Okutangaala | ||||
| Williampulasticity . |
180 |
210 |
260 |
280 |
310 |
| Obukakanyavu (Shorea) . |
42 |
52 |
58 |
68 |
78 |
| Densite(g/cm3) . | 1.11 |
1.14 |
1.17 |
1.20 |
1.22 |
| Amaanyi g’okusika (MPA) . |
9 |
10 |
9 |
9 |
8 |
| okuwanvuwa(%) . | 600 |
550 |
450 |
350 |
250 |
| Amaanyi g’okukutuka (kn/m) . | 18 |
22 |
22 |
22 |
22 |