Telpon: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
PRODUK
Sampeyan kene: Ngarep » Produk » Karet Sintesis Kab » VMQ Silicone » GA-30×1 Silicone rubber for molding (fumed silica) with good anti-yellowing property (HCR)

loading

Share menyang:
tombol enggo bareng facebook
tombol enggo bareng twitter
tombol enggo bareng baris
tombol enggo bareng wechat
tombol enggo bareng linkedin
tombol enggo bareng pinterest
tombol enggo bareng whatsapp
tombol enggo bareng iki

GA-30×1 Silicone rubber for molding (fumed silica) with good anti-yellowing property (HCR)

Aplikasi: macem-macem jinis sarung, peralatan dapur, dompet, jam tangan lan liya-liyane, sing mbutuhake properti anti-kuning sing apik.
Fitur utama: kekuatan dhuwur, transparansi dhuwur, kemampuan proses banget, lulus otentikasi RoHS, REACH, lan LFGB.
  • GA-30×1

kasedhiyan:
Jumlah:

Tes: 1% agen pengawet (50% tempel DBPMH ing permen karet silikon), 175° x5minx15MPa


Parameter produk
produk GA-3021
GA-3031 GA-3041 GA-3051 GA-3061 GA-3071 GA-3081
Penampilan Tembus
Williamplastisitas
100
140
180
210
240
280
310
Kekerasan (ShoreA)
25
30
40
50
60
70
80
Kapadhetan (g/cm3) 1.08
1.08
1.11
1.14
1.17
1.20
1.22
Kekuatan tarik (MPa)

6
8
11
11
11
9
8
Elongasi (%) 950
900
800
700
600
400
200
Kekuwatan sobek (kN/m) 12
18
22
25
30
30
22







Sadurunge: 
Sabanjure: 

LINKS CEPAT

PRODUK KAMI

INFORMASI KONTAK

Tambah: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Telpon / WhatsApp / Skype: +86 15221953351
Hak Cipta     2023 Shanghai Herchy Rubber Co., Ltd. Sitemap |   Kebijakan Privasi | Dhukungan dening Leadong.