GA-60X1F Ultra Heat-resistant Silicone Rubber (300℃)(HCR)

GA-60X1F Ultra Heat-resistant Silicone Rubber ((300℃) (HCR)
Aikace-aikace: dace da samar da auto sassa, zafi jure gadaje, zafi-resistant seals da sauran kayayyakin.
Maɓalli masu mahimmanci: kyakkyawan juriya na zafi da ƙarfin injina, ƙaddamar da amincin RoHS, REACH, da FDA.
  • GA-60X1F

  • Herchy

samuwa:
Yawan:

GA-60X1F Ultra Heat-resistant Silicone Rubber ((300℃) (HCR)


Aikace-aikace: dace da samar da auto sassa, zafi jure gadaje, zafi-resistant seals da sauran kayayyakin.
Maɓalli masu mahimmanci: kyakkyawan juriya na zafi da ƙarfin injina, ƙaddamar da amincin RoHS, REACH, da FDA.
Gwaji: 1% na wakili mai warkarwa (manna 50% na DBPMH a cikin danko silicone), 175°C x 5min x 15MPa.


300 digiri sigogi na samfur
Samfura GA-6041F GA-6051F GA-6061F GA-6071F
Bayyanar Beige
Williamplasticity 150 200 240 240
Hardness ( ShoreA) 40 50 60 70
Girma (g/cm3) 1.14 1.16 1.18 1.2
Ƙarfin ɗaure (MPa) 8.5 9 9.5 9
Tsawaita(%) 700 600 500 400
Ƙarfin hawaye (kN/m) 15 20 25 25
iska tsufa 300 ℃ x70H Tauri 46 63 73 77
Ƙarfin tashin hankali 5.2 5.0 4.9 5.2
Tsawaitawa 350.0 220.0 180.0 160.0


Na baya: 
Na gaba: 

SAUKAR HANYA

KAYANMU

BAYANIN HULDA

Ƙara: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Haƙƙin mallaka     2023 Shanghai Herchy Rubber Co., Ltd. Taswirar yanar gizo |   Manufar Keɓantawa | Taimako Ta Leadong.