GA-60X1F rubair silicone ultra-dhìonach teas ((300 ℃) (HCR)
Iarrtas: Freagarrach airson pàirtean fèin-ghluasadach a dhèanamh, cotan dìon-teas, ròin dìon-teas agus toraidhean eile.
Prìomh fheartan: deagh sheasamh teas agus neart meacanaigeach, cuir seachad dearbhadh RoHS, REACH, agus FDA.
Deuchainn: 1% de stuth-leigheis (50% pas de DBPMH ann an guma silicone), 175 ° C x 5min x 15MPa.
| Paramadairean toraidh 300 ceum | |||||
| Bathar | GA-6041F | GA-6051F | GA-6061F | GA-6071F | |
| Coltas | Beige | ||||
| Williamplasticity | 150 | 200 | 240 | 240 | |
| cruas (CladachA) | 40 | 50 | 60 | 70 | |
| Dlùths (g/cm3) | 1.14 | 1.16 | 1.18 | 1.2 | |
| Neart tensile (MPa) | 8.5 | 9 | 9.5 | 9 | |
| Leudachadh (%) | 700 | 600 | 500 | 400 | |
| Neart deòir (kN/m) | 15 | 20 | 25 | 25 | |
| adhair a 'fàs nas sine 300 ℃ x70H | cruas | 46 | 63 | 73 | 77 |
| Neart teannachaidh | 5.2 | 5.0 | 4.9 | 5.2 | |
| Leudachadh | 350.0 | 220.0 | 180.0 | 160.0 | |