GA-2040
Herchy
| Beskikberens: | |
|---|---|
| Quantity: | |
Test: 130°C x 10min, 200°C x 4H.
| Produkt parameters | |||||
| Produkt | GA-2040-35T |
GA-2040-35 |
GA-2050-35 | GA-2040-45 | |
| Ferskining | Trochsichtich | Griis | Read | Griis | |
| Hardheid (ShoreA) | 35-42 | 35-42 | 48 | 42 | |
| Tichtheid (g/cm 3) | 1.13 |
1.13 |
1.14 |
1.12 |
|
| Treksterkte (MPa) | 9.5 |
9.5 | 9.0 |
9.5 |
|
| Ferlinging (%) | 800 | 800 | 650 | 800 | |
| Tear sterkte (kN/m) | 40 | 40 | 35 |
40 |
|
| Hot leeftyd ferset 153 ° C ± 3 ° C × 7D | Feroaring fan treksterkte (%) | <土10 | <土10 | <土10 | <土10 |
| Feroaring fan ferlinging |
<土10 | <土10 | <土10 | <土10 | |
| Permaninte deformation by konstante útwreiding 300% x 90 ° C x 168H |
<5% | <5% | <5% | <5% | |
| Dielektryske konstante by 100HZ | 3.03 | 3.03 | 3.03 | 2 95 | |
| Dissipaasjefaktor by 100HZ | 0.0029 | 0.0029 | 0.0029 | 0.0029 | |
| Ferset tsjin elektryske lekken en markearring | 1A3.5 | 1A3.5 | 1A3.5 | 1A4.5 | |
| Diëlektryske sterkte (kV/mm) | 24 |
24 |
22 |
23 | |
| Volumeresistiviteit (Ω·cm) | 1.0 *1015 | 1.0 *1015 | 1.0 *1015 | 1.0 *1015 | |