Ga-9442
Herchy
: | |
---|---|
Te rahinga: | |
Whakamatau: DBPMH, te tuatahitanga tuatahi: 170 ° C x 10min, tuku pou.200 ° CICION.200 °.
Nga tohu hua | ||
Hua | Ga-9442 |
Ga-9443 |
Putanga | ngoikore te kowhai |
|
Williammplaticity |
160 |
160 |
Harderss (shorea) |
43 |
43 |
Te whakatauranga (G / CM3) | 1.125 |
1.14 |
Te kaha o te kaha (MPA) |
10.0 |
10.0 |
Elongation (%) | 700 |
700 |
Te kaha haehae (K / M) | 25 |
25 |
Dielectric tonu i te 100hz |
3.03 |
3.03 |
Te wehenga o te 100hz |
0.0029 |
0.0029 |
Te aro turuki | - |
1A3.5 |
Te kaha Dielectric (KV / MM) | 24.3 |
24.3 |
Whakapae rōhi (ω · CM) | 1.0 * 1016 |
1.0 * 1016 |
Whakamatau: DBPMH, te tuatahitanga tuatahi: 170 ° C x 10min, tuku pou.200 ° CICION.200 °.
Nga tohu hua | ||
Hua | Ga-9442 |
Ga-9443 |
Putanga | ngoikore te kowhai |
|
Williammplaticity |
160 |
160 |
Harderss (shorea) |
43 |
43 |
Te whakatauranga (G / CM3) | 1.125 |
1.14 |
Te kaha o te kaha (MPA) |
10.0 |
10.0 |
Elongation (%) | 700 |
700 |
Te kaha haehae (K / M) | 25 |
25 |
Dielectric tonu i te 100hz |
3.03 |
3.03 |
Te wehenga o te 100hz |
0.0029 |
0.0029 |
Te aro turuki | - |
1A3.5 |
Te kaha Dielectric (KV / MM) | 24.3 |
24.3 |
Whakapae rōhi (ω · CM) | 1.0 * 1016 |
1.0 * 1016 |