GA-11×1
Herchy
| Ketersediaan: | |
|---|---|
| Kuantitas: | |
Pengujian: 1% bahan pengawet (50% pasta DBPMH dalam permen karet silikon),175° x 5 menit x 15MPa.
| Parameter produk | ||||||
| Produk | GA-11331 |
GA-1141 | GA-1151 | GA-1161 | GA-1171 | GA-1181 |
| Penampilan | Tembus cahaya | |||||
| Williamplastisitas |
115 |
150 |
205 |
240 |
280 |
260 |
| Kekerasan (ShoreA) |
30 |
40 |
50 |
60 |
70 |
80 |
| Massa jenis (g/cm3) | 1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.23 |
| Kekuatan tarik (MPa) |
7 |
8.5 |
8.5 |
8.5 |
7.5 |
7.5 |
| Pemanjangan(%) | 700 |
550 |
450 |
400 |
300 |
200 |
| Kekuatan sobek (kN/m) | 15 |
19 |
20 |
19 |
19 |
19 |