Ga-93X0 ara ẹni ti a fifin roba (fireeti yanrin) (HCR)

Ohun elo: o dara fun iṣelọpọ ti ohun elo lilẹ ati awọn ọja miiran.
Ẹya bọtini: Ohun-ini ti o dara kikan ti o dara, akoonu epo ti ju 7%, ni afiwe irapada ati arọwọto.
  • Ga-93x0

  • Egbo

Wiwa:
Iwọn:

Idanwo: 1% ti oluran gbigbọn (50% Lẹẹsi ti dbmh ins), 175 ° C X 5min x 15mq X 15Ma.


Ọja Awọn ọja
Ọja Ga-9330 Ga-9340 Ga-9350 Ga-9360 Ga-9370
Ifarahan Milimita
Williaty 140 170 200 220 240
Lile (sheaa) 30 40 50 60 70
Iwuwo (g / cm3) 1.12 1.14 1.17 1.2 1.21
Agbara Tensele (MPA) 9 10 10 8.5 8.5
Piglesation (%) 850 800 700 500 350
Agbara yiya (Kni / M) 20 25 30 25 25


Ti tẹlẹ: 
Itele: 

Awọn ọna asopọ iyara

Awọn ọja wa

IBI IWIFUNNI

Ṣafikun: Bẹẹkọ
Tes / Whatsapp / Skype: +86 15221953351
Aṣẹ-ara     2023 Shanghai Herchy Herchy Co., LtD. Oju-oju opo |   Eto Afihan | Atilẹyin nipasẹ Agbero.