Tel: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
Ngwaahịa
Ị nọ ebe a: Ụlọ GA Ngwaahịa - Rubber Synthesis 10 Silikoni VMQ »» ×3J General purpose silicone roba maka extrusion (HCR)

nbudata

Kekọrịta na:
bọtịnụ nkekọrịta Facebook
bọtịnụ ikesa twitter
bọtịnụ nkekọrịta akara
bọtịnụ nkekọrịta wechat
bọtịnụ njikọ njikọ
bọtịnụ nkekọrịta pinterest
bọtịnụ ịkekọrịta WhatsApp
Kekọrịta bọtịnụ nkekọrịta a

GA-10 × 3J General nzube silicone roba maka extrusion (HCR)

Ngwa: ngwaahịa extrusion nkịtị dị ka o邸narywire, cable, sooks, gluestrip wdg.
Njirimara ndị dị mkpa: ọsọ extrusion ngwa ngwa, ịrụ ọrụ eletrik dị mma, usoro dị mma, gafere nyocha nke RoHS, REACH, na
  • GA-10×3J

  • Herchy

nnweta FDA:
Ọnụ ọgụgụ:

Nnwale: 1.3% nke onye na-agwọ ọrịa (50% tapawa nke DCBP na silicone gum), 130°C x 5min x 15MPa.


Ngwa ngwaahịa
Ngwaahịa GA-3331
GA-3341 GA-3351 GA-3361 GA-3371
Ọdịdị translucent
Williamplasticity
150
215
260
280
310
Isi ike (ShoreA)
42
52
60
70
78
Njupụta (g/cm3) 1.13
1.18
1.19
1.22
1.22
Ike tensile (MPa)

7.5
7.5
7.5
7
7
Mgbatị(%) 550
450
350
250
200
Ike akwa mmiri (kN/m) 16
20
20
20
16








Nke gara aga: 
Osote: 

Njikọ ngwa ngwa

Ngwaahịa anyị

OZI MKPỌTỤRỤ

Tinye: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Nwebiisinka     2023 Shanghai Herchy Rubber Co., Ltd. map saịtị |   Amụma nzuzo | Nkwado Site Leadong.