Tel: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
Ngwaahịa
Ị nọ ebe a: Ụlọ » Ngwaahịa » Rubber Synthesis » FVMQ Fluorosilicone FV9500 Fluorosilicon Rubber

nbudata

Kekọrịta na:
bọtịnụ nkekọrịta Facebook
bọtịnụ ikesa twitter
bọtịnụ nkekọrịta akara
bọtịnụ nkekọrịta wechat
bọtịnụ njikọ njikọ
bọtịnụ nkekọrịta pinterest
bọtịnụ ịkekọrịta WhatsApp
kekọrịta bọtịnụ nkekọrịta a

Fluorosilicon roba FV9500

Ngwaahịa a dabara adaba maka mmepụta ụgbọ ala turbocharger sooks ma ọ bụ ihe ndị ọzọ mejupụtara sooks na ngwaahịa ndị ọzọ.
Ọmarịcha calendering arụmọrụ, co-gwọrọ bonding arụmọrụ na silicone roba
Magburu onwe mmanụ eguzogide, ihe mgbaze.
  • FV9500

  • Herchy

Nnweta:
Ọnụọgụ:

Ngosipụta teknụzụ

Ihe

Ihe ngosi

Ọkwa

FV9540

FV9550

FV9560

FV9561

Ọdịdị

Ụzọ ule

odo odo

Specific ike ndọda/g/cm3

ASTM D792

1.40

1.41

1.42

1.44

Isi ike/ikpere mmiriA

ASTM D2240

41

50

60

61

Ike tensile/MPa

ASTM D412

9.5

9.8

10.2

9.8

Nkwalite na ezumike /%

ASTM D412

370

282

263

310

Ike akwa/KN/m

ASTM D624-B

17

17

18

17

* Okpomọkụ Nguzogide
225 ℃ × 72h

Mgbanwe ike ike / osimiri A

+4

+2

+2

+2

Mgbanwe ike tensile,%

-24

-25

-23

-26

Mgbanwe n'oge mgbanwe, %

-19

-10

-14

-12

Mmanụ ụgbọala C

Mgbanwe olu/%

23 ℃/72h

ASTM D471

+23

+23

+21

+21

Peel Ike/N/mm, ya na rọba silicone methyl vinyl

2.0

2.0

2.2

2.0

Ọnọdụ ọgwụgwọ

Tinye 0.8 akụkụ nke bis-di-quaternary, otu ogbo vulcanisation 120℃×15min, abụọ vulcanisation vulcanisation: 200℃×4h


  • Nguzogide Kasị Elu na gburugburu Harsh : FV9500 fluorosilicone rọba karịrị na gburugburu nwere oke okpomọkụ yana ikpughe na kemịkalụ ike. Ọ na-enye ezigbo nguzogide mmanụ ọkụ, mmanụ, na ụdị kemịkal dị iche iche, na-eme ka ọ dị mma maka ịchọ ngwa ụlọ ọrụ mmepụta ihe.

  • Oke okpomoku zuru oke : ihe a na-enye oke okpomọkụ na-arụ ọrụ sara mbara, site na obere ka -60°C ruo elu ka 200°C. Nke a na-eme ka ọ dị mma maka ngwa n'ime ụgbọ ala, ikuku ikuku, na ụlọ ọrụ mmepụta ihe, ebe mgbanwe okpomọkụ na-adịkarị.

  • Ọkachamara Nguzogide Ntugharị Mkpakọ : FV9500 na-egosipụta nguzogide pụtara ìhè na ntọala mkpakọ, na-ahụ na arụmọrụ ogologo oge yana akara arụmọrụ n'okpuru nrụgide na-adịgide adịgide, ọbụlagodi na ọnọdụ nrụgide dị elu.

  • Ọdịnaya emelitere : Ngwakọta fluorosilicon na-akwalite ịdịte aka megide ịka nká, ozone, na ikpughe UV, na-eme ka ntụkwasị obi na arụmọrụ dị ogologo oge, ọbụlagodi n'okpuru ọnọdụ gburugburu ebe obibi siri ike.

  • Igwe ọkụ eletrik dị elu : Ọ na-enye ihe mkpuchi ọkụ eletrik dị mma, na-eme ka ọ dị mma maka iji ya na ngwa elektrọn yana akara akara ebe nguzogide eletrik dị oke mkpa.

  • Versatility na Ngwa : Enwere ike iji ihe ahụ gafee ụlọ ọrụ dị iche iche, gụnyere ụgbọ ala, ikuku, mmanụ na gas, na ngwá electronic, n'ihi nchikota nke ike n'ibu na nguzogide kemịkalụ.

  • Mgbanwe dị mma na nguzogide mmiri : Fluorosilicone rubber FV9500 na-enye mgbanwe ọbụna na okpomọkụ dị ala, jikọtara ya na akwa akwa akwa na nkwụsị nke abrasion, na-eme ka arụmọrụ a pụrụ ịdabere na ya na ọnọdụ dị ike na nke dị elu.

  • Nhọrọ ọkwa nri dị : Dabere na ihe ị chọrọ, enwere ike ịmepụta ụdị fluorosilicone rubber iji mezuo ụkpụrụ ọkwa nri, na-enye ihe ngwọta dị mma maka ngwa na nhazi nri na ụlọ ọrụ ọgwụ.


Nke gara aga: 
Osote: 

Njikọ ngwa ngwa

Ngwaahịa anyị

OZI MKPỌTỤRỤ

Tinye: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Nwebiisinka     2023 Shanghai Herchy Rubber Co., Ltd. map saịtị |   Amụma nzuzo | Nkwado Site Leadong.