Fluorosilicone Rubber FV9500

Iki gicuruzwa gikwiranye nogukora amamodoka ya turbocharger yimodoka cyangwa ibindi bikoresho byose hamwe nibindi bicuruzwa.
Imikorere myiza ya kalendari, ifatanije gukiza hamwe na silicone reberi
Kurwanya amavuta meza, kurwanya solvent.
  • FV9500

  • Herchy

Kuboneka:
Umubare:

Ibipimo bya tekiniki

Ibintu

Ibipimo

Icyiciro

FV9540

FV9550

FV9560

FV9561

Kugaragara

Uburyo bwo Kwipimisha

umuhondo

Uburemere bwihariye / g / cm3

ASTM D792

1.40

1.41

1.42

1.44

Gukomera / inkombeA

ASTM D2240

41

50

60

61

Imbaraga za Tensile / MPa

ASTM D412

9.5

9.8

10.2

9.8

Kurambura Kuruhuka /%

ASTM D412

370

282

263

310

Imbaraga zamarira / KN / m

ASTM D624-B

17

17

18

17

* Kurwanya Ubushyuhe
225 ℃ × 72h

Guhinduka gukomeye / inkombe A.

+4

+2

+2

+2

Imbaraga zingirakamaro zihinduka,%

-24

-25

-23

-26

Kurambura kuruhuka,%

-19

-10

-14

-12

Ibicanwa C.

Guhindura amajwi /%

23 ℃ / 72h

ASTM D471

+23

+23

+21

+21

Peel Imbaraga / N / mm, hamwe na rebero ya Methyl vinyl silicone

2.0

2.0

2.2

2.0

Gukiza

Ongeramo ibice 0.8 bya bis-di-quaternary, volcanisation yicyiciro kimwe 120 ℃ × 15min, ibirunga byibyiciro bibiri: 200 ℃ × 4h


  • Kurwanya Kurwanya Ibidukikije Bikabije : FV9500 fluorosilicone reberi nziza cyane mubidukikije bifite ubushyuhe bukabije no guhura n’imiti ikaze. Itanga uburyo bwiza bwo kurwanya ibicanwa, amavuta, hamwe n’imiti myinshi, bigatuma biba byiza bisaba inganda.

  • Ubushyuhe bwagutse : Ibi bikoresho bitanga ubushyuhe bwagutse bwo gukora, kuva hasi -60 ° C kugeza kuri 200 ° C. Ibi bituma bikenerwa cyane mubisabwa mumodoka, mu kirere, no mu nganda zikora inganda, aho ihindagurika ry'ubushyuhe risanzwe.

  • Kurwanya Kwiyunvira Byiza Kurwanya : FV9500 yerekana imbaraga zidasanzwe zo guhagarika compression, itanga imikorere igihe kirekire kandi ikanashyiraho ikimenyetso mugihe cyumuvuduko urambye, ndetse no mubihe bikomeye.

  • Kuramba kuramba : Ibigize fluorosilicone byongerera igihe kirekire kurwanya gusaza, ozone, na UV, bigatuma kwizerwa no gukora igihe kirekire, ndetse no mubihe bidukikije bikabije.

  • Isoko ry’amashanyarazi risumba ayandi : Itanga ibikoresho byiza byo gukwirakwiza amashanyarazi, bigatuma biba byiza gukoreshwa mubikoresho bya elegitoronike no gufunga kashe aho kurwanya amashanyarazi ari ngombwa.

  • Guhindura muburyo bukoreshwa : Ibikoresho birashobora gukoreshwa mubikorwa bitandukanye, birimo ibinyabiziga, icyogajuru, peteroli na gaze, hamwe na elegitoroniki, kubera guhuza imbaraga za mashini hamwe no kurwanya imiti.

  • Guhindura neza no Kurira Amarira : Fluorosilicone rubber FV9500 itanga ihinduka nubwo haba hari ubushyuhe buke, ihujwe no kurira neza no kurigata, bigatuma imikorere yizewe mubihe bigenda neza kandi byambaye cyane.

  • Amahitamo yo mu rwego rwibiribwa araboneka : Ukurikije ibyo usabwa, variant ya fluorosilicone reberi irashobora gutegurwa kugirango yujuje ubuziranenge bwibiribwa, itanga igisubizo cyiza kubisabwa mubikorwa byo gutunganya ibiribwa ninganda zimiti.


Mbere: 
Ibikurikira: 

LINKS

IBICURUZWA BYACU

AMAKURU

Ongeraho: No.33, Umuhanda 159, Umuhanda wa Taiye, Akarere ka Fengxian, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Uburenganzira     2023 Shanghai Herchy Rubber Co., Ltd. Ikarita |   Politiki Yibanga | Inkunga Na Kurongora.