Paraiméadair táirge | |||||
Toradh | GA-2041WY | GA-2051WY | GA-2061WY | GA-2071WY | |
Dealramh | Liath liath | Liath liath | Liath dorcha | Liath liath | |
A/bratio |
2: 100 | 2: 100 | 1: 1 | 2: 100 | |
Slaodacht (Pa.S) |
14-20 | 140-160 | 70-90 | 140-160 | |
Cruas (Shorea) | 45 | 50 |
65 |
70 |
|
Dlús (g/cm3) | 1.3 |
1.36 | 1.6 | 1.5 | |
Neart teanntachta (MPA) | 2.5 |
3.0 |
3.0 |
3.0 |
|
Fadú (%) | 200 | 300 | 170 | 140 | |
Neart cuimilte (kn/m) | 7 | 7 | 7 |
8 | |
Aicme lasair |
UL94V-0 | UL94V-0 | UL94V-0 | UL94V-0 |
Tástáil: Tá cóimheas A/B inchoigeartaithe, 130 ° C x 5min x 15MPA
Paraiméadair táirge | |||||
Toradh | GA-2041WY | GA-2051WY | GA-2061WY | GA-2071WY | |
Dealramh | Liath liath | Liath liath | Liath dorcha | Liath liath | |
A/bratio |
2: 100 | 2: 100 | 1: 1 | 2: 100 | |
Slaodacht (Pa.S) |
14-20 | 140-160 | 70-90 | 140-160 | |
Cruas (Shorea) | 45 | 50 |
65 |
70 |
|
Dlús (g/cm3) | 1.3 |
1.36 | 1.6 | 1.5 | |
Neart teanntachta (MPA) | 2.5 |
3.0 |
3.0 |
3.0 |
|
Fadú (%) | 200 | 300 | 170 | 140 | |
Neart cuimilte (kn/m) | 7 | 7 | 7 |
8 | |
Aicme lasair |
UL94V-0 | UL94V-0 | UL94V-0 | UL94V-0 |