| Parameter produk | |||||
| produk | GA-9740 | GA-9750 | GA-9760 | GA-9770 | |
| Penampilan | kulawu | ||||
| Williamplastisitas | 140 | 180 | 200 | 260 | |
| Teu karasa (ShoreA) | 40 | 50 | 60 | 70 | |
| Kapadetan (g/cm3) | 1.23 | 1.25 | 1.28 | 1.32 | |
| Kakuatan tegangan (MPa) | 3.5 | 4.5 | 5 | 5.5 | |
| Elongation(%) | 700 | 600 | 400 | 250 | |
| Kakuatan cimata (kN/m) | 15 | 15 | 15 | 15 | |
| 175'C x22h Komprési(%) | 20 | 20 | 20 | 20 | |
| Sepuh hawa 225°C x70H | Robah karasa | 1 | 2 | 2 | 2 |
| Laju robah kakuatan tegangan | -25% | -25% | -25% | -25% | |
| Laju robah manjang | -30% | -30% | -30% | -30% | |
| IRM903minyak 150°C x70H | Robah karasa | -18 | -18 | -17 | -16 |
| Laju robah kakuatan tegangan | -35% | -35% | -35% | -35% | |
| Laju robah manjang | -20% | -20% | -20% | -20% | |
| Parobahan volume | 36% | 36% | 35% | 35% | |