GA-2002
Herchy
| Helitaanka: | |
|---|---|
| Tirada: | |
Tijaabada: Saamiga A/B ee 1:1, 130°C x 5min x 15MPa
| Xuduudaha alaabta | |||||||
| Alaabta | GA-2002 | GA-2003 | GA-2004 | GA-2005 | GA-2006 | GA-2007 | |
| Muuqashada | Hufan | ||||||
| Adag ( ShoreA) | 23 | 30 | 40 | 50 |
62 |
68 |
|
| Cufnaanta (g/cm3) | 1.10 | 1.12 | 1.12 | 1.13 | 1.14 |
1.14 |
|
| Xoog xajin (MPa) | 6.0 |
8.0 |
9.0 |
9.0 |
10.0 |
9.5 |
|
| Dheeraynta(%) | 750 | 650 | 600 | 500 | 450 |
400 |
|
| Xoogga jeexjeexa (kN/m) | 10 | 15 | 20 |
25 | 30 |
35 |
|
| Waxyaabaha VOC (%) | 0.35 | 0.35 | 0.3 | 0.3 | 0.3 | 0.3 | |