GA-2002
Herchy
| Framboð: | |
|---|---|
| Magn: | |
Próf: A/B hlutfall 1:1, 130°C x 5min x 15MPa
| Vörubreytur | |||||||
| Vara | GA-2002 | GA-2003 | GA-2004 | GA-2005 | GA-2006 | GA-2007 | |
| Útlit | Gegnsætt | ||||||
| hörku (ShoreA) | 23 | 30 | 40 | 50 |
62 |
68 |
|
| Þéttleiki (g/cm3) | 1.10 | 1.12 | 1.12 | 1.13 | 1.14 |
1.14 |
|
| Togstyrkur (MPa) | 6.0 |
8.0 |
9.0 |
9.0 |
10.0 |
9.5 |
|
| Lenging (%) | 750 | 650 | 600 | 500 | 450 |
400 |
|
| Rifstyrkur (kN/m) | 10 | 15 | 20 |
25 | 30 |
35 |
|
| VOC innihald (%) | 0.35 | 0.35 | 0.3 | 0.3 | 0.3 | 0.3 | |