GA-2040
Herchy
| Argaeledd: | |
|---|---|
| Nifer: | |
Prawf: 130 ° C x 10 munud, 200 ° C x 4H.
| Paramedrau cynnyrch | |||||
| Cynnyrch | GA-2040-35T |
GA-2040-35 |
GA-2050-35 | GA-2040-45 | |
| Ymddangosiad | Tryleu | Llwyd | Coch | Llwyd | |
| Caledwch (ShoreA) | 35-42 | 35-42 | 48 | 42 | |
| Dwysedd (g/cm 3) | 1.13 |
1.13 |
1.14 |
1.12 |
|
| Cryfder tynnol (MPa) | 9.5 |
9.5 | 9.0 |
9.5 |
|
| elongation(%) | 800 | 800 | 650 | 800 | |
| Cryfder dagrau (kN/m) | 40 | 40 | 35 |
40 |
|
| Gwrthiant oedran poeth 153 ° C ± 3 ° C × 7D | Newid cryfder tynnol (%) | <土10 | <土10 | <土10 | <土10 |
| Newid elongation |
<土10 | <土10 | <土10 | <土10 | |
| Anffurfiad parhaol ar estyniad cyson 300% x 90°C x 168H |
<5% | <5% | <5% | <5% | |
| Cyson dielectrig ar 100HZ | 3.03 | 3.03 | 3.03 | 2 95 | |
| Ffactor afradu ar 100HZ | 0.0029 | 0.0029 | 0.0029 | 0.0029 | |
| Gwrthwynebiad i ollyngiad trydan a marcio | 1A3.5 | 1A3.5 | 1A3.5 | 1A4.5 | |
| Cryfder Dielectric (kV/mm) | 24 |
24 |
22 |
23 | |
| Gwrthiant Cyfaint (Ω·cm) | 1.0 *1015 | 1.0 *1015 | 1.0 *1015 | 1.0 *1015 | |